Mar 11, 2024 Leave a message

20Cr2Ni4A Heat Treatment: Temperature, Soaking and Case Depth

What 20Cr2Ni4A Is and Where It Fits

20Cr2Ni4A is a high-nickel, chromium-bearing carburising steel listed in GB/T 3077, the Chinese national standard for alloy structural steels. Its carbon content of roughly 0.20% is deliberately low so that the core of a part stays tough after quenching, while 3.25-3.65% nickel and 1.25-1.65% chromium give it hardenability high enough to through-harden sections that would remain soft with a plain 20CrMnTi. The grade is specified for parts that must combine a hard, wear-resistant surface with a core that absorbs shock: heavy-duty gears, pinions, splined shafts, bearing rings for large bearings, crankshafts, connecting rods, hammers, and die-cushion and mining components.

Because the grade is almost always used in the carburised and hardened condition, the phrase "heat treatment temperature" is not a single number. A finished part passes through at least five distinct temperature stages, and the purpose of each is different: normalising after forging, soft annealing for machinability, carburising for carbon pickup, an intermediate high-temperature temper, a final austenitising and quenching step, and a low-temperature temper. Mixing these up, or collapsing them into one, is the most common source of soft cases, excessive retained austenite, distortion and quench cracking in this grade.

Chemical Composition and What the "A" Suffix Changes

Grade limits in GB/T 3077 for 20Cr2Ni4A are commonly quoted as carbon 0.17-0.23%, silicon 0.17-0.37%, manganese 0.30-0.60%, chromium 1.25-1.65% and nickel 3.25-3.65%, with phosphorus and sulphur each held at 0.030% maximum or tighter by agreement. The trailing "A" marks the fine-grain, low-impurity variant: phosphorus and sulphur ceilings are tightened and the steel is deoxidised and grain-refined so that the prior austenite grain size stays fine through a 920-940 °C carburising hold. That matters directly for heat treatment, because a coarse-grain heat will grow austenite grains during carburising, and coarse grains produce a brittle, crack-prone case that cannot be corrected by any subsequent temper.

Element Typical range (%) Influence on heat treatment
C 0.17-0.23 Sets core hardness after quenching; low carbon keeps the core tough
Si 0.17-0.37 Deoxidation; high silicon slightly reduces case carbon uptake
Mn 0.30-0.60 Hardenability and carbide formation in the case
Cr 1.25-1.65 Carbide former; improves case wear resistance and hardenability
Ni 3.25-3.65 Core toughness; also the main cause of retained austenite in the case
P 0.030 max, tighter for the A grade Tramp element; raises temper embrittlement and grain-coarsening risk
S 0.030 max, tighter for the A grade Machinability versus hot ductility; kept low for forging quality
Cu, Sn, Sb, As Residual, normally reported only Collectively raise susceptibility to temper embrittlement

The high nickel content is the defining feature and the defining complication. It suppresses the martensite start temperature, so after quenching from the carburising temperature the case of a 20Cr2Ni4A part can hold 20-35% retained austenite, against a few percent in a 20CrMnTi part. Retained austenite lowers apparent hardness, transforms slowly under load, and causes dimensional drift during service or during later grinding. Every unusual step in the heat-treatment cycle of this grade exists to control that one problem.

The Temperature Map: Five Stages and Their Purposes

The table below gives the working temperature windows used in normal commercial practice for 20Cr2Ni4A. They are process windows, not substitutes for a qualified procedure: the actual values on a shop card depend on section size, furnace type, atmosphere, and the case depth and core hardness the drawing requires.

Stage Temperature Typical hold Purpose and notes
Normalising (after forging) 880-900 °C 1 h per 25 mm of section, air cool Refines the coarse as-forged structure and removes forging stress before machining
Soft annealing / isothermal annealing 650-680 °C 2-4 h, then slow cool Brings delivered hardness down to about 269 HBW max or lower for machining and cold forming
Carburising 920-940 °C Set by case depth, typically 3-8 h at temperature Carbon uptake to 0.75-0.90% at the surface; grain growth must stay controlled
Intermediate high-temperature temper 640-680 °C 3-5 h, often repeated once Destabilises retained austenite and relieves carburising stress before final hardening
Final austenitising and quench 800-830 °C, oil at 60-80 °C 30-60 min at temperature, then quench Dissolves part of the case carbide network without re-dissolving everything; limits austenite retention
Tempering 150-200 °C 2-3 h, air cool Relieves quenching stress, sets final case hardness and dimensional stability

Two numbers in this table are frequently mishandled. First, the final austenitising temperature for a carburised 20Cr2Ni4A part is lower than the core hardening temperature of an uncarburised blank: 800-830 °C rather than 850-880 °C. The lower temperature leaves a proportion of fine alloy carbides undissolved in the case, which limits austenite carbon enrichment and therefore limits retained austenite, while the core still transforms because of its high hardenability. Second, the intermediate temper at 640-680 °C is not optional in this grade. Omitting it and quenching directly from the carburising furnace is the fastest route to a case with 30% or more retained austenite and to cracking during grinding.

Carburising Cycle and Case-Depth Control

Gas carburising at 920-940 °C in a controlled-carbon-potential atmosphere is the standard route, with the carbon potential held around 1.0-1.1% at the boost stage and reduced to about 0.75-0.85% for the diffusion stage so that the surface does not form a brittle carbide network or excessive retained austenite. Boost-diffuse control, rather than a single fixed carbon potential, is what allows a 1.2 mm effective case to be produced without a continuous grain-boundary carbide film at the surface. Atmosphere carbon potential should be monitored continuously and corrected against a dew-point or oxygen-probe reading; a drifting probe is the usual reason two identical loads come out with different case hardness.

Effective case depth is normally specified to the 550 HV1 hardness limit, or as total case depth to the point where hardness stops falling, and is determined on a polished cross-section per GB/T 9450, which corresponds in method to ISO 2639. For gear teeth, case depth is chosen against module: a common rule is 0.15-0.20 times the module for effective case depth, so a module 8 tooth takes roughly 1.2-1.6 mm. For bearing rings and shafts, depth follows the contact-stress calculation instead, and is frequently 1.5-3.0 mm. Overshooting case depth is not a safe choice: an over-carburised case is brittle in bending, holds more retained austenite, and increases the risk of case crushing and of cracking under press fits.

Intergranular oxidation and non-martensitic surface layers also deserve a limit on the drawing. At 920-940 °C, chromium and alloying elements oxidise along grain boundaries to a depth of 10-25 microns in air-containing atmospheres, and that layer will not harden. A specification that caps intergranular oxidation at 15-20 microns forces the heat treater to control gas composition properly instead of relying on a post-grind allowance that may not exist.

Why the Intermediate High-Temperature Temper Is Essential

After carburising, the case of 20Cr2Ni4A consists of martensite, fine alloy carbides and a substantial amount of retained austenite, because the high nickel content pushes the martensite finish temperature far below room temperature. If the part is simply reheated and quenched again, part of that austenite survives and the case never reaches its intended hardness. The standard remedy is a tempering hold in the 640-680 °C range for three to five hours: at that temperature the retained austenite decomposes into ferrite and carbide, the carbon in solution drops, and the case's alloy carbides coarsen slightly into a distribution that dissolves only partially during the final 800-830 °C austenitising hold. The result is a case that transforms more completely on quenching and holds far less austenite.

The same hold relieves the stresses built up by the carburising cycle and by the slow cooling through the martensite range, which reduces distortion in the final quench. For demanding parts, the intermediate temper is applied twice, with an intermediate cool to below 100 °C, because the transformation of retained austenite is time- and temperature-dependent and a single hold can leave islands untransformed. Where dimensional stability is critical, such as precision gears and spindle components, the sequence is completed with a sub-zero treatment at about -60 to -80 °C after the final quench and before tempering; this transforms the remaining austenite and is followed immediately by the 150-200 °C temper to avoid fresh cracking.

Final Austenitising, Quenching Medium and Section Size

The austenitising step is short by design. A hold of 30-60 minutes at 800-830 °C after the part reaches temperature is enough for these sections, and a long soak at the upper end of the window re-dissolves case carbides and pushes retained austenite back up. Quenching is in oil, and the oil should be held at 60-80 °C with controlled agitation: warm, moderately fast oil gives the cooling rate needed through the case without the thermal shock of water. Water quenching of this grade is not acceptable practice. The combination of a hard, thin case on a tough core, plus high hardenability, produces a steep stress gradient during cooling, and water quenching reliably produces quench cracks at section changes, keyways, and oil holes.

Section size changes the picture less than for a low-hardenability grade, because 20Cr2Ni4A hardens deeply: oil-quenched bars of 50-80 mm diameter can be substantially martensitic at the centre, and even heavier sections harden through the case and a large part of the core. The practical consequence is that the core is strong but not very ductile if the section is large, and the heat treater must choose between a core hardness target and toughness. Typical as-quenched core hardness after the 800-830 °C oil quench falls in the 35-45 HRC band for medium sections, and the tempering temperature is then used to bring it down to the drawing requirement, usually 30-40 HRC for gears and shafts.

Tempering, Distortion and Crack Avoidance

Tempering after the final quench should start within two hours, before the part reaches room temperature in cold weather or within a few hours at most. Delayed tempering of a high-carbon case is a recognised cause of delayed quench cracking, and the risk is highest at fillets and at the bottom of keyways where the case is thin. A 150-200 °C hold of two to three hours at temperature, followed by air cooling, gives the usual 58-62 HRC case with acceptably low retained austenite and relieves enough stress to make grinding safe. Raising the tempering temperature above about 250 °C starts to soften the case measurably and is only appropriate where the drawing allows a lower surface hardness.

Distortion control in this grade is mostly a matter of fixture and handling discipline rather than of temperature. Parts should be quenched in fixtures that support thin sections, oriented so that oil flows symmetrically, and never dropped into the quench tank in a bundle. Machining allowance must account for the dimensional change from the retained-austenite transformation: a case that stabilises over the following days will grow slightly, so critical diameters are often left with grinding stock and finished after a stabilising hold. Straightening after quenching is a high-risk operation on a carburised case and should be done warm, at 150-200 °C, never cold.

Acceptance Testing and Documentation

Acceptance of a heat-treated 20Cr2Ni4A part rests on destructive and non-destructive evidence that should be specified on the drawing rather than agreed after delivery. The usual set is: surface hardness on the finished surface, a hardness traverse on a sectioned coupon to establish effective case depth at the 550 HV1 limit, a core hardness reading at a defined depth, a metallographic check for carbide network, retained austenite level and intergranular oxidation depth, and a check that no softening or decarburisation remains on functional surfaces. Rockwell testing follows GB/T 230.1 and Vickers testing GB/T 4340.1; case-depth determination follows GB/T 9450.

For gear work, material and heat-treatment quality grades are commonly taken from GB/T 3480.5, which defines allowable stress values linked to documented microstructure and hardness control. A heat treater claiming a high quality grade must be able to show the corresponding records: furnace temperature uniformity survey, atmosphere calibration, load charts, and coupon results traceable to the load. The material certificate to GB/T 3077 covers the steel, not the heat treatment, and a common documentation gap is a delivery with a mill certificate for the bar and no evidence at all for the carburising and hardening cycle.

FAQ

Q: What is the quenching temperature for 20Cr2Ni4A?
For an uncarburised blank the hardening temperature is normally 850-880 °C, but for a carburised part the final austenitising temperature is lower, typically 800-830 °C, followed by oil quenching at 60-80 °C.

Q: Why must 20Cr2Ni4A be tempered at 640-680 °C after carburising?
The high nickel content leaves 20-35% retained austenite in the case after carburising. A 640-680 °C hold decomposes that austenite and precipitates carbides, so the case transforms more fully during the final quench and retains far less austenite.

Q: What case depth is used for 20Cr2Ni4A gears?
Effective case depth is commonly set at about 0.15-0.20 times the gear module, measured to the 550 HV1 limit per GB/T 9450, so a module 8 tooth takes roughly 1.2-1.6 mm.

Q: Can 20Cr2Ni4A be water quenched?
No. The combination of high hardenability and a hard case on a tough core makes water quenching a common cause of quench cracking at section changes, keyways and oil holes; warm oil with controlled agitation is the standard medium.

Q: What surface hardness can be expected after carburising and hardening?
A carburised, quenched and tempered 20Cr2Ni4A case is normally specified and achieved at 58-62 HRC, with the core brought to roughly 30-40 HRC depending on section size and tempering temperature.

Q: Is sub-zero treatment necessary for 20Cr2Ni4A?
It is not mandatory for general parts, but a hold at about -60 to -80 °C after quenching and before tempering is used where dimensional stability matters, because it transforms the remaining austenite that would otherwise cause slow size change in service.

Send Inquiry

whatsapp

phone

Email

Inquiry