Mar 26, 2024 Leave a message

25CrMo4 Alloy Steel: 1.7218 Chemistry, Hardening and Welding

What 25CrMo4 Designates

25CrMo4 is a low-alloy chromium-molybdenum steel for quenching and tempering, standardised in EN 10083-3 under material number 1.7218. The designation follows the European rule of nominal alloy content: approximately 0.25 percent carbon, about 1 percent chromium and a small molybdenum addition of roughly 0.2 percent, the last digit grouping indicating the carbon level in hundredths. Its closest North American equivalent is AISI or SAE 4130, and the nearest designation in GB/T 3077 is 25CrMo. All three describe the same metallurgical concept, though the permitted ranges and the testing regime differ between the standards, so equivalence should be judged on composition and mechanical results rather than on the name alone.

One persistent error circulates in secondary sources: that 25CrMo4 contains 25 percent chromium, 0.80 percent molybdenum and 0.90 percent carbon. Such an analysis describes a high-chromium tool or heat-resistant steel, not this grade, and would be neither forgeable nor weldable in the way 25CrMo4 is used. The real chromium range is roughly one percent and the carbon range is around a quarter of one percent. A purchaser who receives a certificate showing chromium above 1.5 percent or carbon above 0.35 percent should reject it as a different material, regardless of the grade name printed on the document.

The commercial significance of the grade is its position between plain carbon steel and the higher-alloyed 42CrMo4. The chromium and molybdenum pair raises hardenability and temper resistance without pushing carbon equivalent so high that welding becomes impractical, which is why 25CrMo4 appears in thin-walled tube structures, forged fittings, automotive and motorsport components, and pressure parts that must be joined by welding after machining.

Chemical Composition Under EN 10083-3

The standard composition window is narrow enough that small variations in carbon decide the outcome of heat treatment. The ranges below reflect the EN 10083-3 specification for 25CrMo4; product analysis tolerances apply within the limits permitted by that standard.

Element Specified range, % Metallurgical function
Carbon 0.22 - 0.29 Sets the attainable hardness after quenching
Silicon 0.40 max Deoxidation; contributes to solid solution strengthening
Manganese 0.60 - 0.90 Hardenability and sulphur control through manganese sulphide
Phosphorus 0.025 max Restricted for toughness and temper embrittlement resistance
Sulphur 0.035 max Free-machining variants raise this and add controlled inclusions
Chromium 0.90 - 1.20 Hardenability, temper resistance, modest corrosion resistance
Molybdenum 0.15 - 0.30 Suppresses temper embrittlement, raises high-temperature strength

Carbon equivalent calculated on the composition above falls near 0.65 using the conventional formula, which places the grade firmly in the range where preheat and controlled cooling are mandatory for welding rather than optional. Sulphur deserves separate attention: the standard grade with sulphur at the upper end machines more freely but loses ductility in the short-transverse direction, while a resulphurised free-cutting variant is a different product and should not be used for a dynamically loaded part without an engineering decision.

Mechanical Properties in the Quenched and Tempered Condition

The properties that matter commercially are those delivered in the quenched and tempered condition, usually written as +QT. EN 10083-3 grades the requirements by ruling section, because a 200 mm bar cannot be hardened through its centre to the same level as a 16 mm bar regardless of chemistry. The figures below show the general pattern of the specification across section sizes.

Ruling section Tensile strength, MPa 0.2% proof strength, MPa Elongation, %
16 mm and below 800 - 950 635 min 16 min
Over 16 mm to 40 mm 750 - 900 590 min 14 min
Over 40 mm to 100 mm 700 - 850 490 min 15 min
Over 100 mm to 160 mm 650 - 800 400 min 16 min

Impact energy requirements follow the same size grading, with the specification normally quoting a minimum absorbed energy from Charpy V-notch specimens tested at room temperature. The grade is not intended as a low-temperature steel: where service temperature drops below roughly minus 20 degrees Celsius, the design should move to a nickel-bearing or fine-grained steel with a certified transition curve rather than rely on 25CrMo4 at reduced temperature.

In the annealed or normalised condition the grade is much softer, with tensile strength around 600 to 750 MPa after normalising and hardness in the region of 200 HB. Suppliers sometimes quote normalised properties while the drawing calls for +QT, so every certificate should state the delivery condition unambiguously alongside the test results.

Hardenability and Section Size

The chromium and molybdenum combination gives 25CrMo4 adequate through-hardening in oil up to roughly 25 mm section, with the depth decreasing as the quenching medium becomes milder. Above that size, hardness falls progressively from the surface to the core, and the resulting microstructure is a mixture of martensite, bainite and, in heavy sections, ferrite and pearlite. That gradient is not a defect; it is a design input, because the properties at the quarter-point rather than at the surface govern the performance of a large forged component.

Hardenability is characterised by the Jominy end-quench test to ISO 642 or ASTM A255, and a purchaser of bar for a critical part is entitled to ask for the hardenability band rather than a single composition. Two heats inside the same composition window can differ by several millimetres in the depth at which hardness falls to 50 HRC, and that difference changes distortion, residual stress and fatigue performance in a part that is subsequently ground.

For thick sections the alternative to a more severe quench is a more highly alloyed grade. Water quenching 25CrMo4 above 60 mm raises the risk of quench cracking and excessive distortion, particularly in parts with sharp section changes, so the usual engineering answer is to accept lower core properties, to specify 42CrMo4, or to redesign the section.

Heat Treatment Windows

Soft annealing is carried out near 700 to 720 degrees Celsius followed by slow cooling, producing a spheroidised structure with hardness around 200 HB maximum and good machinability. Stress relieving after rough machining uses a temperature below the eventual tempering temperature, typically 600 to 650 degrees Celsius, so that the subsequent hardening treatment does not disturb the relief achieved.

Hardening takes place from an austenitising temperature in the region of 850 to 880 degrees Celsius, with a soak of roughly one hour per 25 mm of section and oil quenching as the default medium. The upper part of the range dissolves more carbon and raises hardness but also coarsens the austenitic grain, which increases distortion and reduces toughness in the finished part. A grain size check on the austenitising practice, or a requirement for fine grain steel, is a cheap safeguard against a coarse-grained heat.

Tempering is the step where the grade earns its reputation. Held between 540 and 680 degrees Celsius and cooled in air, the part develops a tempered martensite structure with a good balance of strength and ductility. Tempering in the 250 to 400 degrees Celsius band should be avoided: that window produces tempered martensite embrittlement, visible as a drop in impact energy despite an acceptable tensile result, and the damage cannot be recovered by a subsequent higher temper in every case. Molybdenum in the grade delays temper embrittlement during slow cooling from the tempering temperature, which is the reason the addition is present at all.

Machining and Forming

In the soft annealed or normalised condition 25CrMo4 machines readily with carbide tooling at conventional speeds, while the quenched and tempered condition at 800 to 950 MPa demands reduced cutting speed, rigid setups and attention to tool edge preparation. Because the grade work-hardens only mildly, finish passes should remove a consistent depth of cut rather than skim the surface, which otherwise produces a worked layer that interferes with subsequent grinding or Nitriding-type surface treatments.

Cold forming of tube and sheet is practical within limits. 25CrMo4 tubing for structural frames is commonly cold drawn and then stress relieved, and bent sections should be annealed or normalised after severe deformation before heat treatment. Hot forming is carried out in the 850 to 1100 degrees Celsius range with a finishing temperature high enough to avoid working in the two-phase region, followed by normalising to refine the structure.

Decarburisation during hot working or heat treatment is a real risk. A decarburised layer on a part that will be quenched leaves a soft skin that fails to develop martensite and can initiate fatigue cracks under bending. Purchasers of bar for highly stressed parts should specify the permitted decarburisation depth, test it by microscopic examination of a transverse section, and allow sufficient machining stock to remove it.

Welding 25CrMo4

25CrMo4 is weldable but not forgiving. The carbon equivalent near 0.65 means the heat-affected zone will harden rapidly on cooling unless heat input and cooling rate are controlled, and the risk of hydrogen-assisted cold cracking is significant in thick sections and in restrained joints. Preheat of 150 to 250 degrees Celsius, scaled to thickness and to the ambient temperature of the workshop, is standard practice rather than an optional refinement.

Consumables should under-match the parent metal strength rather than match it. A filler depositing roughly 550 to 620 MPa tensile strength, such as a 1.2 percent chromium-molybdenum type classified in the appropriate AWS specification, gives a weld metal with better toughness and lower crack sensitivity than a matching 800 MPa deposit. Low-hydrogen consumables, clean and dry joint faces and a controlled interpass temperature complete the basic package.

Post-weld heat treatment at 550 to 650 degrees Celsius, applied after the weld has cooled, relieves residual stress and tempers the hardened zone. The soak should not be skipped for thin sections either, because restraint rather than thickness governs cracking. Welding procedure qualification to ISO 15614-1 or ASME BPVC Section IX, with hardness traverses across the heat-affected zone and impact tests where the service demands them, is the appropriate evidence that the combination of preheat, filler and heat treatment actually works for the specific joint.

Product Forms and Related Standards

Bar and rod are supplied to EN 10083-3 in the European system and to ASTM A29/A29M or ASTM A322 where the North American designation 4130 is used. Seamless mechanical tubing for structural and pressure applications is commonly ordered to ASTM A519 in 4130, while aerospace users work to AMS 6370, which adds cleanliness, grain size and hardenability requirements beyond the general bar standard. Open-die forgings in the grade are covered by EN 10250-3.

The differences between these documents are not administrative. AMS 6370 imposes tighter limits on non-metallic inclusions and requires hardenability response to be demonstrated, which matters for a forged aircraft fitting but is unnecessary for a general machined bushing. Ordering to the correct standard is cheaper than discovering at first article inspection that the certificate does not carry the cleanliness rating the drawing implies.

Applications and Grade Selection

The best-known use of 25CrMo4 is thin-walled tubular structures: bicycle frames, motorsport chassis, aircraft engine mounts, and landing gear components on light aircraft, where a high strength-to-weight ratio is achieved with wall thicknesses of one or two millimetres. In these applications the steel is usually supplied in the cold drawn and stress relieved condition, welded with a low-carbon filler, and the joint design rather than the material limits the load.

In heavier engineering the grade serves for hydraulic cylinder components, gear blanks, shafting, bolts and studs for elevated temperature service, drill string subs, and pump and valve bodies. Its temper resistance keeps strength at temperatures where a plain carbon quenched and tempered steel would soften, so components that run warm, such as exhaust-adjacent brackets or steam fittings, benefit from the molybdenum addition.

Selection against neighbouring grades is straightforward once the service is defined. Where maximum strength in a moderate section is needed and welding is not involved, 42CrMo4 delivers more. Where the part is welded and the section is thin, the lower carbon of 25CrMo4 is a genuine advantage. Where service temperature exceeds roughly 450 degrees Celsius for long periods, a creep-resistant chromium-molybdenum grade with a documented elevated temperature dataset is required instead.

Inspection and Acceptance Points

A certificate for 25CrMo4 should state the delivery condition, the ruling section used for the mechanical tests, the heat analysis, and the results of tensile and impact testing. Where the part is safety-related, the purchaser should add a hardenability requirement, a non-metallic inclusion rating to a recognised method, a grain size assessment, and a decarburisation limit. Hardness testing across a section is a fast confirmation that the specified heat treatment actually reached the core of the component rather than only its surface.

Three acceptance failures recur. The first is a certificate showing tensile strength above the specified range, which usually indicates an under-tempered part rather than a superior one. The second is a composition with carbon at the upper limit in a part that will be welded, which pushes carbon equivalent and cracking risk up without any gain in the design allowables. The third is a mismatch between the standard quoted on the drawing and the standard quoted on the certificate, most often 4130 bar supplied against a European drawing that calls for EN 10083-3 without a documented equivalence review.

Storage and Handling

Bar and tube should be stored under cover, off the ground, with ends protected against mechanical damage that would later appear as a machining defect. Quenched and tempered bar is sensitive to impact at edges, and a bruised or nicked surface can act as a stress raiser in a part that is subsequently loaded in bending. Bundles should be separated by size and heat number so that traceability survives into the machine shop, and any cut remnant returned to stock should be re-marked with its heat number rather than left unidentified.

FAQ

Q: Does 25CrMo4 contain 25 percent chromium?
No. The 25 refers to approximately 0.25 percent carbon, and chromium is specified between 0.90 and 1.20 percent. A certificate showing chromium near 25 percent describes a completely different steel.

Q: Is 25CrMo4 identical to AISI 4130?
They are close equivalents, but the composition windows and the testing requirements differ between EN 10083-3 and the ASTM or AMS documents. Treat them as interchangeable only after comparing actual composition limits and mechanical results for the form being purchased.

Q: What is the correct tempering temperature for 25CrMo4?
Between roughly 540 and 680 degrees Celsius for a quenched and tempered structure, selected by the strength level required. Tempering between 250 and 400 degrees Celsius should be avoided because of tempered martensite embrittlement.

Q: Why is preheat needed before welding?
The carbon equivalent near 0.65 causes the heat-affected zone to harden on cooling, and combined with diffusible hydrogen this produces cold cracking under restraint. Preheat of 150 to 250 degrees Celsius plus low-hydrogen consumables and post-weld heat treatment controls the risk.

Q: Can 25CrMo4 be used for pressure tubing?
Yes, seamless tube in the 4130 designation is widely used for mechanical and pressure tubing to ASTM A519, provided the design pressure and temperature are supported by the specified mechanical properties and the welding procedure is qualified for the actual joint.

Q: Does 25CrMo4 resist corrosion?
Only mildly. The chromium content is far too low to form a passive layer, so the grade rusts in ambient conditions and requires painting, oiling or plating. It does offer better resistance than plain carbon steel in mildly aggressive industrial atmospheres, but it is not a stainless steel.

Send Inquiry

whatsapp

phone

Email

Inquiry