Mar 12, 2024 Leave a message

50CrMo4 (1.7228) Quenched and Tempered Alloy Steel Plate

What 50CrMo4 Is and Where It Sits in the Quenched and Tempered Family

50CrMo4, designated 1.7228 in the European numbering system, is a medium-carbon chromium-molybdenum alloy steel supplied in the quenched and tempered condition under EN 10083-3. With roughly 0.50 % carbon, 1 % chromium and 0.2 % molybdenum, it sits at the high-strength end of the wrought quenched and tempered family: stronger than 42CrMo4 (1.7225) and considerably stronger than 34CrMo4 (1.7220), but with correspondingly lower ductility and a much narrower heat-treatment window. In the American designation system it is closest to AISI 4150, and in the Japanese system to the SCM 4 series, although the exact limits differ and substitution should always be checked element by element rather than by grade name.

The alloy is chosen when a component has to carry a high load in a section thick enough that a plain carbon steel would not harden through. Chromium raises hardenability and contributes wear resistance through carbide formation; molybdenum suppresses temper embrittlement and delays the bainite transformation, which is what allows oil quenching of sections in the 50–100 mm range without cracking. The result is a steel that can be tempered anywhere between about 28 and 55 HRC from a single austenitising treatment, which makes it a general-purpose strong steel rather than a single-purpose one.

Chemical Composition and the Standard Framework

Under EN 10083-3 the grade is controlled on heat analysis with product analysis tolerances applied to the ladle result. The composition window is deliberately tight on carbon because hardness after tempering is dominated by carbon content: a 0.04 % drift at the top of the range shifts the tempered hardness by several HRC at a fixed tempering temperature, which is enough to fail a hardness specification.

Element EN 10083-3 range (mass %) Effect on processing and service
C 0.46–0.54 Sets achievable hardness and strength; upper half improves wear resistance but reduces toughness and weldability
Si 0.40 max Deoxidation; excessive silicon promotes temper embrittlement and surface decarburisation
Mn 0.50–0.80 Hardenability; combines with sulphur, so manganese and sulphur limits must be read together
P 0.025 max Segregation and temper embrittlement; the single most damaging residual element in this grade
S 0.035 max Free-machining benefit at the cost of anisotropy and toughness
Cr 0.90–1.20 Hardenability and carbide former; improves resistance to softening on tempering
Mo 0.15–0.30 Retards bainite, suppresses temper embrittlement, raises high-temperature strength
Cu + Sn 0.30 max / 0.05 max typical Tramp elements from scrap; raise embrittlement risk and are usually capped by agreement

Two practical points follow from this table. First, the carbon range is narrow enough that the difference between a compliant and a non-compliant heat is sometimes only visible in the mechanical test, so the mill certificate must be read for the actual value rather than the grade name. Second, molybdenum at 0.15–0.30 % is the element that distinguishes this grade from a plain 1 % chromium steel, and it is precisely the element that most affects behaviour during slow cooling and during elevated-temperature service.

Mechanical Properties and How Section Size Changes Them

Quenched and tempered properties in EN 10083-3 are tabulated against the ruling section of the product, because hardenability - not composition alone - decides what the centre of a bar or plate actually achieves. A 25 mm plate quenched in oil transforms almost fully to martensite and tempers to a uniform structure. A 150 mm plate of the same heat may retain bainite or fine pearlite at mid-thickness, and the tensile test taken from the quarter position will show lower strength and markedly lower toughness than the surface.

Ruling section Indicative tensile strength Rm (MPa) Indicative yield strength Re (MPa) Indicative elongation A (%) Typical hardness after tempering
≤ 16 mm 1100–1300 ≥ 900 ≥ 10 32–38 HRC
16–40 mm 1000–1200 ≥ 850 ≥ 11 30–36 HRC
40–100 mm 900–1100 ≥ 750 ≥ 12 28–34 HRC
100–160 mm 800–950 ≥ 650 ≥ 13 26–31 HRC
160–250 mm 750–900 ≥ 550 ≥ 14 24–29 HRC

The figures above are indicative ranges for the quenched and tempered delivery condition and are intended for grade comparison; the binding values for a specific order are those tabulated for the ordered section and inspection condition. The direction of the trend, however, is fixed and matters more than any single number: for every doubling of section thickness, expect a step down in achievable strength and a step up in the scatter of impact energy.

Impact toughness deserves separate attention. At 0 °C a properly quenched and tempered 50CrMo4 section of moderate thickness typically delivers Charpy V-notch energy in the 30–60 J range, but the same steel tempered to the same hardness in a 200 mm section may fall below 20 J because the centreline structure is not fully martensitic. Specifying impact energy without specifying the test position is one of the most common causes of disputed deliveries in this grade.

Hardenability and Why Section Size Decides the Grade

The ideal critical diameter of 50CrMo4 in oil is approximately 50–70 mm, which is to say that a round bar of that diameter will harden to at least 80 % martensite at the centre under ideal quenching. In practice, real quench severity is lower than ideal: still oil in a small tank, poor agitation and heavy scale all reduce the effective cooling rate, so the working limit for full through-hardening is usually quoted at 40–60 mm depending on the quenching installation.

Above that limit the steel still works, but the design assumption has to change. Instead of expecting uniform martensite, the designer accepts a mixed structure and specifies properties from the quarter-thickness position. Where full through-hardness is essential in a heavy section, the correct response is either to move to a higher-hardenability grade (more chromium and molybdenum, plus nickel) or to accept a lower strength level. Increasing the austenitising temperature to force deeper hardening is the wrong response: it coarsens the grain, increases distortion and quench-crack risk, and gains very little.

Grain size control is the other half of the hardenability story. A fine prior-austenite grain size of ASTM 7 or finer keeps the martensite packet small, which raises both toughness and the resistance to quench cracking. Aluminium-killed fine-grain practice is therefore standard, and a coarse-grain heat will fail impact requirements even when chemistry and hardness are correct.

The Heat Treatment Sequence

There is no solution treatment in the processing route of this steel. It is a wrought, homogenised product delivered in the quenched and tempered condition, and any additional thermal cycle should be planned as a normalise, austenitise, quench and temper sequence. The correct sequence for a component machined from plate or bar is as follows.

Normalising at 870–900 °C, holding one hour per 25 mm of section, then air cooling, refines a structure that has been disturbed by forging or heavy machining and gives a uniform starting point. It is optional for plate already supplied in a controlled condition, but essential after any hot forming operation.

Austenitising for hardening is carried out at 840–880 °C. The lower half of that range is preferred for fine-grain control and minimum distortion; the upper half is used only when the section is heavy and the furnace load is large. Soak time at temperature should be about 20–30 minutes per 25 mm of section once the load is through, not the hour per 25 mm used for normalising, because a long hold at 860 °C coarsens grain and deepens decarburisation.

Quenching is normally in agitated oil at 40–80 °C. The quench must be fast enough to miss the pearlite and bainite noses but not so violent that it generates cracking in a complex shape. Polymer quenchants are used where oil would be a fire risk, but their cooling curves must be measured rather than assumed, because a polymer concentration that drifts upward will quietly leave a bainitic core. Parts should be quenched to below about 100 °C before removal, then tempered immediately - a delay of even a few hours at room temperature after quenching is enough to produce quench cracks in sections with sharp changes of thickness.

Tempering follows as soon as the part reaches 50–80 °C, with a soak of at least one hour per 25 mm of section and a full air cool afterwards.

Tempering temperature Indicative hardness (HRC) Indicative Rm (MPa) Typical use of that condition
As quenched 57–62 - Not a service condition; too brittle for structural use
180–220 °C 53–57 1800–2000 Wear surfaces, tools, lightly loaded dies
300 °C 48–52 1650–1800 Transition zone to be avoided for critical parts
400 °C 42–46 1400–1550 High-strength shafts with moderate toughness demand
500 °C 38–42 1250–1400 Heavily loaded gears, connecting components
550 °C 34–38 1100–1250 General quenched and tempered structural parts
600 °C 30–34 1000–1100 Parts needing impact resistance over strength
650 °C 27–31 900–1000 Maximum toughness, pressure-retaining components

These hardness values are indicative for a fully martensitic section; a partially hardened core will read lower at every tempering temperature, and the gap widens as the tempering temperature falls.

Tempering, Embrittlement and the Temperatures to Avoid

Two embrittlement mechanisms govern the choice of tempering temperature in this grade, and both are aggravated by phosphorus, tin and antimony in the steel.

The first is temper brittleness in the 250–400 °C range, where tempered martensite embrittlement reduces impact energy sharply without any visible change in hardness or tensile strength. A part tempered at 300 °C can show half the Charpy energy of the same part tempered at either 200 °C or 450 °C. Since hardness falls monotonically with tempering temperature, this creates a trap: the hardness target may be met at 300 °C, but the toughness at that condition is worse than at a higher temperature with a slightly lower hardness.

The second is temper embrittlement on slow cooling from above 500 °C. If a part is tempered at 600 °C and cools slowly through the 400–550 °C band - for example, inside a furnace or in a large stacked load - phosphorus and tin segregate to prior-austenite grain boundaries and the ductile-to-brittle transition temperature shifts upward by 30–80 °C. The remedy is straightforward: water or forced-air cool from the tempering temperature for any section where impact toughness matters, and hold phosphorus at the low end of the specification. Molybdenum at 0.15–0.30 % is the reason this grade tolerates slow cooling better than a plain chromium steel, but it does not make the practice safe in heavy sections.

A third practical rule concerns multiple tempering. Double tempering is used for large or complex parts to ensure the entire section has been held at temperature; the second temper is normally 10–20 °C below the first and serves mainly to temper any retained austenite that transformed on cooling from the first temper.

Welding, Machining and Surface Treatment

At 0.46–0.54 % carbon this is not a weldable steel in the structural sense. Arc welding without preheat will produce a hard, crack-sensitive heat-affected zone with a carbon equivalent well above 0.60, and hydrogen-assisted cold cracking follows within hours. Where welding is unavoidable, the correct approach is to preheat the whole component to 200–250 °C, use low-hydrogen consumables dried to the manufacturer's schedule, maintain the preheat through the operation, and perform a post-weld heat treatment at 550–620 °C immediately after welding rather than allowing the part to cool. Even then, the joint will not match the base-metal strength, and the design should not rely on it doing so.

Machining is best done in the annealed or normalised condition, or after a softening temper, because the quenched and tempered condition at 30–38 HRC is hard on carbide tooling. For finishing after hardening, cubic boron nitride or ceramic inserts are required, and the depth of cut must stay below the decarburised layer, which can be 0.2–0.5 mm deep. Ignoring that layer is a common cause of a part that measures correctly with a portable hardness tester and then wears prematurely, because the soft skin is only a few tenths of a millimetre thick.

For surface hardening, induction or flame hardening of 50CrMo4 is feasible and produces a case of 55–60 HRC to a depth of 2–6 mm over a tough core. Nitriding is also used, but only after quenching and tempering, and the tempering temperature must exceed the nitriding temperature by at least 30 °C to prevent the core from softening during the nitriding cycle. That single rule eliminates most nitriding failures in this grade.

Applications and Substitution Logic

The combination of high strength, moderate through-hardening capability and reasonable elevated-temperature stability places 50CrMo4 in heavy mechanical engineering rather than in mass-produced parts. Typical uses include large shafts and axles for crushers and mills, gear blanks and ring gears in industrial drives, connecting rods and pins in heavy machinery, mould and die holders in injection moulding, pressure-retaining components for moderate-temperature service, and drill-string or tool components where a combination of strength and wear resistance is needed.

Substitution should be driven by the section size and the strength target rather than by grade familiarity. Where the section is under 40 mm and 1000 MPa tensile strength is sufficient, 42CrMo4 will do the same job with better ductility and lower cracking risk. Where the section exceeds about 60 mm and full through-hardness is required, a higher-hardenability grade with nickel is usually cheaper than attempting to force 50CrMo4 to harden. Where elevated-temperature strength above 400 °C is the governing requirement, a chromium-molybdenum steel with higher molybdenum or a different alloy family should be considered instead.

The one substitution that should be avoided is replacing 50CrMo4 with a case-hardening or plain carbon steel on the basis of similar hardness. Hardness equivalence says nothing about the distribution of that hardness through the section, and it says nothing about tempering resistance in service.

Buyer Verification: Certificates, Tests and Tolerances

A delivery of 50CrMo4 plate or bar should be accompanied by an inspection certificate to EN 10204 type 3.1, giving the actual heat analysis, the heat treatment condition and the mechanical test results with the test position stated. The following checks catch nearly all of the deviations that matter.

Check Reference What to confirm
Heat analysis EN 10083-3 limits, EN 10204 3.1 Carbon and molybdenum inside the window; phosphorus at the low end; tramp elements capped
Tensile test EN ISO 6892-1 Rm, Re and elongation consistent with the ordered ruling section, test position stated
Impact test EN ISO 148-1, Charpy V Test temperature, specimen orientation and notch position all specified in the order
Hardness survey EN ISO 6506 (Brinell) or 6507 (Vickers) Measured below the decarburised layer, with a documented traverse for heavy sections
Ultrasonic test EN 10160 Class agreed for the application; internal discontinuities in heavy plate are a real risk
Grain size EN ISO 643 ASTM 5 or finer; a coarse-grain heat will not meet impact requirements
Dimensions EN 10029 for plate, EN 10060 for bar Thickness tolerance class, flatness and edge condition
Surface Visual and dimensional No quench cracks, grinding burn or deep scale pits; decarburisation depth measured

When a part fails in service, the first question is almost always whether it was fully hardened at the position where it failed. A through-thickness hardness traverse on a section cut from the failed part answers that question in an hour and is far more informative than repeating the tensile test.

Common Processing Errors

Treating 50CrMo4 as a stainless or high-alloy grade and applying a solution treatment at 1000–1050 °C is wrong and damaging. At that temperature the grain grows rapidly, the surface decarburises deeply, and the subsequent quench produces a coarse, crack-prone martensite. There is no solid-solution step in this steel's route; the correct austenitising range is 840–880 °C.

Tempering at 150–250 °C to reach a high hardness and calling the result quenched and tempered is also a misapplication. That condition is a hardened-and-slightly-tempered state suitable only for wear surfaces with light loading. Components required to carry load and absorb impact need tempering at 500–650 °C, accepting 27–42 HRC in exchange for ductility and toughness.

Quenching a thick section in still oil without agitation, and then accepting the hardness reading from the surface, hides a soft core. Surface hardness is the least informative single measurement for this grade; a traverse from surface to centre is the only way to confirm that the intended structure was actually produced.

Finally, grinding a hardened part without coolant control produces untempered martensite in a surface layer a few hundredths of a millimetre thick. That layer is harder than the specification, brittle, and in a cyclic-load application it becomes the crack initiation site. Pickling or a controlled temper after grinding removes most of the risk.

FAQ

Q: What is the difference between 50CrMo4 and 42CrMo4?
Both are chromium-molybdenum quenched and tempered steels under EN 10083-3, but 50CrMo4 carries 0.46–0.54 % carbon against 0.38–0.45 % for 42CrMo4. The higher carbon gives roughly 100–150 MPa more tensile strength at the same tempering temperature, at the cost of lower elongation, lower impact energy and a greater risk of quench cracking.

Q: What is the correct austenitising temperature for hardening 50CrMo4?
840–880 °C, with a soak of about 20–30 minutes per 25 mm of section, followed by an agitated oil quench. Temperatures above 900 °C coarsen the grain and deepen decarburisation without improving hardenability enough to justify the damage.

Q: Which tempering temperatures should be avoided?
The 250–400 °C band, where tempered martensite embrittlement sharply reduces impact energy with no change in hardness, and slow cooling through 400–550 °C after tempering above 500 °C, which causes temper embrittlement. Water or forced-air cooling from the temper avoids the second problem.

Q: Can 50CrMo4 be welded?
Only with a controlled procedure: preheat to 200–250 °C, low-hydrogen consumables, and immediate post-weld heat treatment at 550–620 °C. The carbon equivalent exceeds 0.60, so cold cracking is a real risk without these measures, and the joint will not match base-metal strength.

Q: How deep does decarburisation go after heat treatment?
Typically 0.2–0.5 mm on an unprotected surface, depending on furnace atmosphere and time at temperature. It must be removed by machining before service, and hardness testing must be taken below it to give a meaningful reading.

Q: What does 1.7228 mean and is it the same as 50CrMo4?
1.7228 is the numerical designation used in the European steel numbering system for the grade sold as 50CrMo4. The two designations describe the same steel, so a certificate quoting either is acceptable provided the composition and condition match EN 10083-3.