Mar 19, 2024 Leave a message

20MnCr5 Alloy Structural Steel Plate: Composition and Application Fields

What 20MnCr5 Plate Is

20MnCr5 is a manganese-chromium case-hardening steel defined in EN 10084. It is a low-carbon alloy grade with a nominal carbon content of about 0.20 %, 1.10-1.40 % manganese and 1.00-1.30 % chromium, supplied as hot-rolled plate, sheet or bar for parts that will be carburised, hardened and tempered. The combination of a machinable, tough core with a hard case is the reason the grade is widely used for gears and bearing components.

Chemical Composition to EN 10084

Element Limit, % (heat analysis)
C 0.17-0.22
Si 0.40 max
Mn 1.10-1.40
P 0.035 max
S 0.035 max
Cr 1.00-1.30

Manganese and chromium raise hardenability, so the grade can be quenched in sections much thicker than plain carbon case-hardening steels at the same carbon level. Sulphur and phosphorus are capped at 0.035 % each because inclusion content controls fatigue life in dynamically loaded teeth and races.

Case Hardening and Heat Treatment Behaviour

Typical practice is carburising at 900-950 C, quenching, and tempering at 150-200 C. Surface hardness after hardening is usually 58-62 HRC, while the core remains in the range of roughly 30-42 HRC, equivalent to about 1000-1300 MPa tensile strength depending on hardenability and quenching medium. Effective case depth is set by the component design, most often 0.6-1.5 mm, and is verified on sectioned coupons rather than on the finished part. Because core strength is developed in the same quench as the case, distortion must be allowed for in the machining sequence.

Application Fields

Transmission gears. Gears for automotive and industrial gearboxes, reducers and power take-offs work at high surface pressure and depend on both the hard case and the tough core of 20MnCr5.

Bearing rings. Outer and inner rings of roller and ball bearings, where the grade provides a hard raceway and a core that resists spalling under repeated rolling contact.

Construction and earthmoving machinery. Pins, bushes, sprockets, hydraulic pump parts and transmission components for excavators and loaders that see shock loading and abrasive dust.

Moulds and dies. Injection moulds, die-casting inserts and punches requiring a wear-resistant surface backed by a tough substrate.

Standards and Equivalent Grades

EN 10084 is the reference specification for the grade and fixes the composition limits and hardenability band. In Chinese practice the nearest alloy structural steel is 20CrMn, and comparable manganese-chromium case-hardening chemistries are used in US and Japanese practice. Plate is normally supplied to EN 10029 dimensional tolerances, and internal soundness can be verified by ultrasonic examination to ASTM A578/A578M when the order requires it.

Fabrication Notes

Machinability in the soft annealed condition is good, with hardness typically around 170-220 HB. Welding is not recommended on finished components: 1.10-1.40 % Mn and 1.00-1.30 % Cr raise hardenability and the carbon level is not balanced for weldability, so local hardening and cracking are likely without preheat and post-weld heat treatment. Where a joint cannot be avoided, a low-hydrogen consumable, controlled preheat and immediate post-weld treatment are required, and the joint should be kept outside the carburised zone.

Frequently Asked Questions

Q: Which standard covers 20MnCr5?
A: EN 10084 covers the grade as a case-hardening steel with controlled core composition rather than a guaranteed delivery strength.

Q: What is the nominal carbon content?
A: 0.17-0.22 % carbon, balanced with 1.10-1.40 % Mn and 1.00-1.30 % Cr for hardenability.

Q: What case depth is used for gears?
A: Most gears run with an effective case depth of 0.6-1.5 mm, derived from the module and the contact stress.

Q: Can the plate be welded?
A: Only with a qualified procedure, preheat and post-weld heat treatment; the grade is designed for carburising rather than for welded fabrication.

Q: Is heat treatment included in the delivery condition?
A: No. Plate is supplied annealed or as-rolled for subsequent machining, carburising, quenching and tempering.

Q: Why are sulphur and phosphorus limited?
A: Both are capped at 0.035 % because non-metallic inclusions reduce fatigue life in gear teeth and bearing rings.

Send Inquiry

whatsapp

phone

Email

Inquiry