DNV Grade E
DNV Grade E is an ordinary-strength shipbuilding steel plate used for building ship hulls and marine structures. It offers good toughness, adequate strength, corrosion resistance, and excellent welding performance. The grade is specified by the classification society DNV (Det Norske Veritas) and is suitable for ships operating in coastal, river, and cold ocean waters, although higher grades such as EH36 are used for harsher, low-temperature environments. The E designation indicates Charpy impact testing at -40 degrees Celsius.
Chemical Composition
The chemical composition of DNV Grade E is specified with maximum limits of carbon 0.18 percent, phosphorus 0.035 percent, and sulfur 0.035 percent, with silicon in the range 0.10-0.35 percent and manganese at 0.70 percent maximum. A minimum aluminum content of 0.015 percent supports fine-grain practice, which contributes to the grade's toughness. The controlled carbon and impurity levels make the plate easy to weld by conventional shipyard processes.
Mechanical Properties
The mechanical properties of DNV Grade E are verified by thickness range. For thickness up to 50 mm, the minimum yield strength is 235 MPa, tensile strength 400-520 MPa, elongation at least 22 percent, and Charpy V-notch impact energy at -40 degrees Celsius at least 20 J for energy 1 and 27 J for energy 2. For thickness above 50 mm up to 70 mm, the impact requirement rises to 24 J and 34 J. For thickness above 70 mm up to 150 mm, it rises further to 27 J and 41 J.
Equivalent Grades
DNV Grade E has equivalents in other classification societies, including ABS Grade E (AB/E), GL Grade E (GL-E), LR Grade E (LR/E), BV Grade E (BV/E), CCS Grade E (CCS/E), NK Grade E (K E), KR Grade E (R E), and RINA Grade E (RI/E). Although the grades share a similar strength and toughness level, the governing rules of each society differ in detail, so equivalence should be confirmed against the specific class notation required by the project.
Applications
DNV Grade E plates are used for ship hulls and structures, including the shell plating, decks, and bulkheads of vessels operating in coastal, river, and cold ocean waters. The grade's combination of weldability, toughness, and moderate strength makes it a practical choice for ordinary-strength shipbuilding applications, while high-strength and low-temperature grades are selected where design loads or service temperatures demand more.
Frequently Asked Questions
What does E mean in DNV Grade E? The E designation indicates Charpy impact testing at minus 40 degrees Celsius.
What is the yield strength of DNV Grade E? 235 MPa minimum, with tensile strength 400-520 MPa and elongation at least 22 percent.
What are the equivalents of DNV Grade E? B/E (ABS), GL-E, LR/E, BV/E, CCS/E, K E (NK), R E (KR) and RI/E (RINA).
Where is it used? Hulls and structures of ships operating in coastal, river and cold ocean waters.
What thickness ranges are covered? Up to 50 mm, 50-70 mm and 70-150 mm, with impact energy rising from 20/27 J to 27/41 J.
Is DNV Grade E weldable? Yes, it has excellent welding performance with conventional shipyard processes.