Nov 22, 2023 Leave a message

FH36 Steel Plate: Minus 60 C Toughness and Class Rules

Reading the FH36 Grade Symbol

FH36 is a fully killed, fine grain, higher strength hull structural steel plate. The symbol is built from three separate decisions that the shipyard, the designer and the steel mill each have to agree on. The first letter fixes the impact test temperature: A denotes testing at 0 degrees C, D at minus 20, E at minus 40 and F at minus 60 degrees C. The letter H states that the plate belongs to the higher strength series rather than the normal strength series. The number 36 gives the nominal minimum yield strength in kilogram-force per square millimetre, so FH36 corresponds to a minimum yield of 355 MPa in SI terms.

F grade therefore means the toughest impact requirement in the common hull structural family, and FH36 is ordered for the parts of a vessel where thick plate, high restraint and a low design temperature coincide: ice classed hulls, deck and bottom plating in the forward region, hatch coamings, crane pedestals, and heavy brackets where a brittle fracture would propagate. The related grades AH36, DH36 and EH36 share the same strength and chemistry framework and differ mainly in impact temperature, so the same mill may roll all four from similar heats with different processing and testing.

Chemical Composition and Micro-Alloy Design

The grade relies on a low carbon, fine grain approach with niobium, vanadium, titanium and aluminium additions rather than on high carbon content. The table below gives the composition frame normally applied to higher strength hull plate; the actual limits that bind a given order are those in the classification society rule set named in the purchase order.

Element Typical limit for FH36 plate Technical purpose
C 0.18% max (often 0.16% max for thick plate) Strength; kept low to protect toughness and weldability
Si 0.10 - 0.50% Deoxidation
Mn 0.90 - 1.60% Strength and toughness balance
P 0.035% max Residual; low to avoid segregation and brittleness
S 0.035% max Residual; controls sulphide inclusion shape
Al (acid soluble) 0.015% min Fine grain practice through aluminium nitride
Nb, V, Ti Micro-alloy additions, subject to carbon equivalent control Grain refinement and precipitation strengthening
Cu, Cr, Ni Residual or deliberate additions, restricted by rule set Corrosion resistance or toughness, depending on grade variant

Carbon equivalent is the number that decides whether a thick plate can be welded without preheat. A 60 mm FH36 plate with a carbon equivalent near the upper limit of a rule set requires preheat and a controlled heat input that a 15 mm plate of the same grade does not. Buyers should require the carbon equivalent value, calculated to the formula named in the applicable rule set, to appear on the mill certificate for every heat, because it drives fabrication cost far more than the headline yield strength does.

Mechanical Properties and the Minus 60 Degree Impact Test

FH36 combines a 355 MPa minimum yield with a tensile range typically 490 to 620 MPa and good elongation, but the property that defines the grade is the Charpy V-notch absorbed energy at minus 60 degrees C. The standard requirement is a minimum of 47 J average for the common hull structural series, and higher strength F grades are frequently ordered to 60 J to satisfy a particular rule set or an ice class notation. Testing is normally transverse to the rolling direction, from a specified position related to the plate thickness.

Property Typical requirement Notes
Yield strength ReH 355 MPa min Transverse tensile specimen
Tensile strength Rm 490 - 620 MPa Upper limit keeps weld metal matching manageable
Elongation A 21% min (thickness dependent) Gauge length per rule set
Charpy V-notch, minus 60 C 47 J min average, 60 J commonly specified Transverse set of three specimens
Carbon equivalent Per rule set formula, typically 0.38 - 0.42 for thick plate Drives preheat and heat input limits
Through thickness (Z) quality Z15 / Z25 / Z35 on request Per GB/T 5313 reduction of area criteria

Thickness matters to all of these numbers. A 100 mm section cannot be rolled and cooled at the same rate as a 12 mm plate, so the mill compensates with a lower carbon level, a tighter carbon equivalent and thermomechanical processing. When an order mixes thin and thick plate of nominally the same grade, expect different processing routes and inspect the thick items more closely for toughness scatter.

Delivery Condition: As Rolled, Normalized or Thermomechanically Rolled

Hull structural plate of this strength class is supplied in one of three conditions, and the condition is part of the grade, not a finishing option. Normalized delivery involves austenitizing, holding and air cooling, producing a uniform ferrite-pearlite structure with predictable toughness across heavy sections; it is the traditional route for thick F grade plate. Thermomechanically controlled rolling achieves the same strength by controlled deformation and accelerated cooling, refining the grain without a separate heat treatment, and is the common route for medium thickness. As rolled delivery is used for thinner plate where the rolling schedule alone gives the required properties.

Fabricators must not normalize thermomechanically rolled plate to "improve" it. A reheat above the tempering range coarsens the structure that the controlled rolling produced and can drop the minus 60 degree impact energy below the acceptance value, invalidating the certification. Where post-weld heat treatment is required by the design, discuss it with the mill before ordering and confirm the allowable treatment temperature and holding time.

Welding FH36 Without Losing the Toughness

Welding is where an FH36 plate most often loses the properties that were paid for. Three parameters control the outcome: preheat, heat input and consumable selection. Preheat depends on carbon equivalent, plate thickness and the ambient humidity of the yard, and rule sets give minimum values that should be treated as a floor rather than a target. Heat input should stay within the range used in the qualified procedure: too high a heat input coarsens the heat affected zone, too low a heat input raises hardness and hydrogen cracking risk in thick restrained joints.

Consumables for 355 MPa class hull steel are generally matching strength, low hydrogen types, baked and stored in heated quivers. For F grade work, the weld metal itself should show adequate Charpy energy at the design temperature, and the procedure qualification should include impact tests of weld metal and heat affected zone at minus 60 degrees C rather than only at the plate test temperature. Where a joint is highly restrained, a crack tip opening displacement test may be required by the designer, and that test is far cheaper to plan at the procedure stage than to add after fabrication has begun.

Practical yard rules: keep groove faces dry and free of mill scale before welding, avoid repairing the same location repeatedly because each thermal cycle further degrades the heat affected zone, and record repair locations and procedures so that an inspector can verify that the number of repairs stays within the rule set's limit.

Z-Direction Quality, Laminations and Ultrasonic Inspection

Thick hull plate in tee joints and block connections is loaded through its thickness, and the weakness that shows up there is a lamination or an inclusion cluster parallel to the surface. Two defences apply. First, order through thickness property quality to Z15, Z25 or Z35 where the design calls for it; GB/T 5313 defines these by minimum reduction of area in a tensile test taken in the short transverse direction, and the higher the Z value the cleaner and more isotropic the plate must be. Second, order ultrasonic testing to a defined acceptance level, either per a national standard such as GB/T 2970 or per the classification society's own instruction, and specify the level and the coverage rather than simply writing "UT" on the order.

Ultrasonic inspection is also the tool that catches internal discontinuities before they turn into weld repairs. Specify whether the whole plate or only the edges and the tee joint zones are scanned, and require the report to travel with the plate rather than arriving separately, since plates and reports are frequently separated in a stockyard.

Class Approval, Certification and Documentation

Hull structural steel is not certified by the mill alone. The plate must be approved and, where the yard is building to class, individually surveyed by the classification society named in the contract. The major societies operating in international shipbuilding are CCS, ABS, DNV, BV, LR, NK, KR and RINA, and each publishes its own rule requirements for chemical composition, mechanical testing, freedom from defects and marking. FH36 plate can be supplied with several society approvals from the same heat where the composition and test regime satisfy all of them, which is common practice for stock material.

Required documentation typically includes the mill certificate with heat number, product analysis, tensile and impact results with test temperatures, the delivery condition, the class approval stamp or certificate number, and the marking transferred to the plate. Until the shipyard's inspection department confirms these items, the plate is not released to production, so document errors are schedule risks and not clerical details. National standards such as GB/T 712 for hull structural steel and ASTM A131/A131M in the ASTM system describe the same family of grades and are commonly cited alongside the rule set.

Ordering Specification Checklist

A purchase order that avoids disputes states the grade and impact class, the rule set and society approval, the delivery condition, the thickness range with tolerances, the through thickness quality if required, the ultrasonic inspection level and coverage, the carbon equivalent limit, the certificate type and the marking requirement. Where plate will be cut into nested parts, also state the requirement on edge condition and on the location of any coil or slab welds, and confirm whether the plate may carry repair welds at the mill.

On receipt, verify the heat number against the certificate before cutting, confirm the class stamp, and check thickness at several points across the width rather than at one location. Store plate clear of the ground on dunnage with drainage, and keep F grade plate segregated so that a nominally similar A or D grade plate cannot be picked for an F grade part. That single storage discipline prevents the most expensive error in a hull steel stockyard.

FAQ

Q: What does FH36 mean in shipbuilding steel?
F fixes the Charpy impact test temperature at minus 60 degrees C, H indicates the higher strength series, and 36 gives the nominal minimum yield strength, equivalent to 355 MPa in SI units.

Q: What is the difference between EH36 and FH36?
The strength level and chemistry framework are essentially the same; the difference is the impact test temperature, minus 40 degrees C for EH36 and minus 60 degrees C for FH36, so FH36 is chosen where the design temperature or the ice class demands greater toughness.

Q: Can FH36 plate be normalized after thermomechanical rolling?
Generally it should not be, because a reheat above the tempering range coarsens the refined structure produced by controlled rolling and can reduce impact energy below the acceptance value. Any post-weld heat treatment must be agreed with the mill in advance.

Q: What carbon equivalent is acceptable for FH36?
There is no single number; each classification society rule set gives a formula and a limit, commonly in the region of 0.38 to 0.42 for thick plate. The value should be declared on the mill certificate for every heat because it determines preheat and heat input.

Q: What does Z35 quality add to an FH36 order?
Z35 is a through thickness property requirement defined in GB/T 5313 by minimum reduction of area in the short transverse direction, which forces cleaner steel with fewer laminations for tee joints and other connections loaded through the plate thickness.

Q: Which documents should accompany each FH36 plate?
A mill certificate with heat number, product analysis, tensile and impact results at the specified temperature, carbon equivalent and delivery condition, together with the classification society approval marking and any ultrasonic inspection report specified in the order.

Send Inquiry