What SA516 Gr.70 Plate Is and Where It Sits in the Pressure Vessel Standards
SA516 Gr.70 is a carbon-silicon killed steel plate produced to ASTM A516/A516M, the specification covering pressure vessel plates for moderate and lower temperature service. In ASME construction the same product is ordered as SA516 Gr.70 under Section II Part A, and the two designations differ only in the administrative route of acceptance: ASTM A516/A516M is the material specification, while ASME SA516 inherits it together with the general requirements of ASTM A20/A20M and the ASME code rules for welding, heat treatment and impact testing.
The grade number "70" is not a strength class in megapascals; it refers to the specified minimum tensile strength of 70 ksi, which converts to approximately 485 MPa. Because of that dual-unit origin, drawings often state tensile strength as 70/90 ksi, or equivalently 485/620 MPa, and purchasers should insist that the mill test certificate states the unit system actually used for testing. Gr.70 is the highest of the four standard carbon grades in the A516 series (Gr.55, Gr.60, Gr.65 and Gr.70) and is the grade normally selected when wall thickness driven by pressure or by stiffness would otherwise push a Gr.60 design into a heavier plate.
In ASME Section II Part D the SA516 series is tabulated for service up to about 343 degrees C (650 degrees F). Above that ceiling the allowable stress falls away and chromium-molybdenum grades such as SA387 become the correct choice. At the low end, the grade is not a cryogenic material in its own right: impact testing is not mandatory in the base specification, and low-temperature qualification only exists when supplementary toughness requirements are ordered or when the ASME UCS-66 curve exemption is satisfied for the actual thickness and stress ratio.
Chemical Composition Requirements
A516/A516M controls chemistry by ladle analysis with product tolerances taken from A20/A20M. Carbon is capped as a function of thickness so that thick sections retain weldability and toughness; manganese is deliberately held in a band rather than a simple maximum, because both strength and notch toughness depend on it. The table below summarises the Gr.70 limits that appear on virtually every purchase order.
| Element | Limit (% by ladle analysis) | Practical note for buyers |
|---|---|---|
| C | 0.27 max up to 12.5 mm; 0.28 max over 12.5 to 50 mm; 0.30 max over 50 to 100 mm; 0.31 max above 100 mm | Carbon equivalent drives preheat and PWHT decisions; ask for CE on every heat |
| Mn | 0.85-1.20 | Upper part of the band is normal for 50 mm and heavier plate |
| Si | 0.15-0.40 | Indicates killed steel; low Si values point to a different deoxidation route |
| P | 0.035 max | 0.025 max or 0.020 max is a common refining purchase requirement |
| S | 0.035 max | 0.010 max or 0.005 max for HIC-resistant orders |
| Al (acid soluble) | 0.020 min when fine grain practice is specified | Fine grain practice is required for normalised thick plate |
| Cu, Ni, Cr, Mo | Reported; each typically 0.30 max as residual | Residuals above these levels are treated as alloy additions and change the P-Number |
| V, Nb, Ti | 0.02 / 0.01 / 0.03 max as residual | Any deliberate microalloying takes the plate out of plain A516 scope |
Two things are routinely got wrong on incoming inspection. First, the carbon limit is thickness dependent, so a certificate for 10 mm plate cannot be used to justify a 60 mm heat. Second, the residual limits for Cr, Cu, Ni and Mo are not "alloying intent" limits, but once they are exceeded the material no longer behaves as P-No.1 in ASME welding procedure qualification, which invalidates an existing WPS without any change to the grade stamp.
Mechanical Properties and the Thickness Effect
Tensile requirements are stated as a range, not a minimum, because A516 plate is expected to be soft enough to form. For Gr.70 the specified tensile strength is 485-620 MPa (70-90 ksi) and the minimum yield strength is 260 MPa (38 ksi) for plate up to 50 mm, with elongation measured on a 200 mm gauge length of 17 percent minimum or 21 percent on a 50 mm gauge length, depending on which test specimen the specification edition in force requires.
| Property | Requirement (Gr.70, plate up to 50 mm) | Comment |
|---|---|---|
| Tensile strength, Rm | 485-620 MPa (70-90 ksi) | Both limits are mandatory; over-strength plate is a rejection item |
| Yield strength, ReH | 260 MPa min (38 ksi) | Yield is not the design driver for most vessel shells |
| Elongation | 21% min (50 mm gauge) / 17% min (200 mm gauge) | Formability indicator for heads and shells |
| Reduction of area | Not specified in the base grade | Order as a supplementary requirement if the design needs it |
| Hardness | Not specified in the base grade | Usually imposed separately for sour service or weld Procedural Qualification |
Thickness matters in a second, less obvious way. A516/A516M requires plate thicker than 40 mm (1.5 in) to be supplied in the normalised condition, and normalising raises yield slightly while improving toughness scatter from heat to heat. Designers who calculate allowable stress from a table entry derived for thin plate, then order 80 mm plate, should expect the mill to deliver normalised material with a different thermal history and a different residual stress state, which in turn changes distortion behaviour during rolling and welding.
Delivery Condition, Normalising and Heat Treatment
The default delivery condition depends on thickness and on what the purchaser writes on the order. Three states are common in the market:
As-rolled or controlled rolled for thin plate where the design is exempt from impact testing under UCS-66 and no normalising is required by the specification.
Normalised for plate above 40 mm, and for any thickness where the purchaser needs a stable, fine-grained microstructure for low-temperature service or for consistent response to post-weld heat treatment.
Normalised plus stress relieved where the fabricator wants to reduce residual stress before cutting and forming, or where a simulated PWHT test coupon must represent the final vessel condition.
Normalising is carried out in the range 900-940 degrees C with a hold of roughly one hour per 25 mm of section, followed by air cooling. Post-weld heat treatment for P-No.1 carbon steel normally sits between 595 and 650 degrees C, with a minimum holding time of one hour and one hour per 25 mm of thickness thereafter. The critical acceptance point is not the nominal temperature but the recorded chart: buyers should require furnace charts with load thermocouples, because a plate that was "stress relieved" at 560 degrees C has not received the treatment the design assumed.
For welded pressure parts, the test coupon that demonstrates mechanical properties after heat treatment must be given the same or a longer thermal cycle than the production weld. This is the single most common source of dispute when a fabricator shortens the PWHT hold to save furnace time and then finds the Charpy results in the procedure qualification report no longer represent the vessel.
Impact Toughness, Sour Service and Supplementary Requirements
The base A516 grade does not mandate Charpy V-notch testing, which is why two identical certificates can describe very different materials. Toughness enters through three separate routes:
Supplementary requirements of A20/A20M ordered by the purchaser, most commonly the Charpy V-notch requirement, vacuum treatment, restricted chemistry and product analysis options.
ASME UCS-66 impact test exemption curves, which link minimum design metal temperature to nominal thickness and to the ratio of design stress to allowable stress. A 25 mm shell stressed to one third of allowable can be exempt well below zero; a 75 mm shell at full allowable cannot.
Project specifications that impose a minimum absorbed energy at a stated temperature, for example 27 J average at minus 20 degrees C, with a defined testing frequency per heat and per thickness range.
For wet hydrogen sulphide service the plate is usually ordered with hardness control and with resistance testing. Hydrogen induced cracking is evaluated to NACE TM0284 and sulphide stress cracking to NACE TM0177, with acceptance criteria set by the end user rather than by A516 itself. Because HIC resistance depends on sulphur level, calcium treatment and centreline segregation, such orders must specify S 0.005 percent maximum or 0.002 percent maximum together with a thickness-direction test if the plate will carry through-thickness stress.
Ultrasonic examination is another discretionary item. ASTM A435 covers straight-beam examination of pressure vessel plates, while ASTM A578 is used where a tighter acceptance class is needed for critical vessels. Z-direction ductility, expressed as a through-thickness reduction of area in the Z15, Z25 or Z35 quality classes, is ordered where welded nozzles and attachments impose lamellar tearing risk.
Plate Dimensions, Tolerances and Edge Preparation
Dimensions and tolerances are governed by A20/A20M rather than by the A516 text itself. Thickness tolerance is expressed as a permitted minus deviation under nominal thickness for plate ordered to nominal thickness, and the allowed deviation widens as thickness increases. Width and length tolerances, camber and flatness are all separately tabulated, and flatness is the tolerance most often missed at goods-in because it is judged visually instead of against a straight edge and feeler gauge.
Common commercial formats for Gr.70 are 2000 mm, 2200 mm and 2500 mm width with 6000 mm to 12000 mm length, or cut-to-size blanks for head pressing. Where heads are to be formed, the purchaser should state the forming direction relative to the rolling direction, since transverse properties govern the crown of a dished head, and should add a forming allowance for the thinning that occurs at the knuckle.
Edge condition also deserves a line on the order. Sheared edges on plate above about 12 mm leave a cold-worked, hardened zone that can initiate cracking during rolling; thermal cutting followed by grinding of the cut face is the usual specification for shell courses and for any edge that will be welded without further preparation. Weld edge preparation angles, root faces and the removal of the mill scale in the weld zone belong in the fabrication drawing rather than in the material order.
Welding and Fabrication Practice
A516 Gr.70 welds readily with the processes used for carbon steel pressure equipment: shielded metal arc with E7018 electrodes, submerged arc with F7A2 or F7A4 flux-electrode combinations, gas metal arc and flux cored arc. The governing variables are carbon equivalent, restraint and hydrogen input, not the process name.
Carbon equivalent calculated as C + Mn/6 + (Cr + Mo + V)/5 + (Ni + Cu)/15 should be held at 0.45 or below for thick or highly restrained joints. Below 25 mm and with a CE under 0.40, preheat of 50 to 100 degrees C is normally sufficient; above 40 mm, or where CE approaches 0.45, preheat of 100 to 150 degrees C and a minimum interpass temperature should be written into the welding procedure. Hydrogen control matters more than nominal preheat: basic coated low-hydrogen electrodes must be held in a drying oven at the manufacturer's stated temperature and issued in heated quivers, and submerged arc fluxes must be baked before use.
Post-weld heat treatment follows ASME UCS-56 for P-No.1 material, with the requirement triggered above 32 mm nominal thickness for the general case unless a specific exemption applies. During PWHT the plate softens slightly, tensile strength falls by roughly 20 to 40 MPa and the Charpy transition temperature shifts upward; procedure qualification coupons must therefore be heat treated with the production cycle, not with an approximation of it.
Applications and Selection Logic
Gr.70 dominates the carbon steel shell market because it satisfies the largest number of vessel designs with a single grade. Typical uses include compressed air and nitrogen receivers, LPG and ammonia storage vessels operating in the moderate temperature band, process drums, knockout drums, heat exchanger shells, column skirts and sumps, plus a long list of non-code general engineering fabrications that adopt A516 simply because the plate is readily available with full certification.
The selection logic is straightforward. Compare Gr.60 and Gr.70 on required thickness at the design pressure and temperature, then compare the resulting weights, welding hours and PWHT costs. Gr.70 usually wins when the shell is 12 mm or more at the Gr.60 condition, because each millimetre saved reduces weld volume as well as plate weight. Gr.60 remains the better choice for very thick, highly restrained or sour service joints where the lower carbon and manganese ceilings make toughness and hardness easier to control.
Three application traps recur. Using Gr.70 above 343 degrees C without checking the allowable stress in Section II Part D; assuming that the plate is impact tested because the vessel is, without ordering the supplementary requirement; and accepting a certificate that reports only tensile properties when the design relies on a toughness exemption. Each of these is a documentation problem rather than a metallurgical one, and each is cheap to prevent at the order stage.
Purchasing and Inspection Checklist
State the specification edition, the grade, and whether ASME or ASTM acceptance is required.
State thickness with the tolerance basis, plus width, length and quantity in pieces and in tonnes.
State delivery condition: as-rolled, normalised, or normalised and stress relieved, with the heat treatment parameters to be recorded.
State the impact testing requirement explicitly: test temperature, absorbed energy, specimen orientation and testing frequency.
State ultrasonic examination class, Z-quality class and any hardness or HIC requirement.
Require mill test certificates with heat number, ladle and product analysis, carbon equivalent, heat treatment records and, where applicable, simulated PWHT data.
Require plate identification by heat number on each piece, with the stamping or marking method agreed so that marking does not create notch-like stress raisers on the surface.
Agree the dimensional verification method, including flatness measurement with a straight edge, and the acceptance sampling plan for thickness at several points per plate.
At goods-in, the practical sequence is: verify heat number continuity between plate marking and certificate, check thickness at a minimum of five points, check flatness and edge condition, confirm the delivery condition against the furnace chart, and confirm that any impact or UT report carries the correct heat and thickness range. A plate that fails any of these checks should be quarantined before cutting, because once a shell course is rolled, the material cannot be returned to the mill on a documentation defect.
FAQ
Q: What is the difference between SA516 Gr.70 and A516 Gr.70?
A516 Gr.70 is the ASTM designation and SA516 Gr.70 is the ASME code designation for the same plate; the ASME version adds code acceptance, marking and heat treatment rules on top of the ASTM chemistry and tensile requirements.
Q: Is SA516 Gr.70 supplied normalised as standard?
Only above 40 mm nominal thickness, where A516/A516M requires normalising. Thinner plate is normally as-rolled or controlled rolled unless normalising is written on the order.
Q: Does SA516 Gr.70 require Charpy impact testing?
No, not in the base grade. Toughness must be ordered as a supplementary requirement or justified through the ASME UCS-66 exemption curve for the actual thickness and stress ratio.
Q: What is the maximum service temperature for SA516 Gr.70?
Approximately 343 degrees C (650 degrees F) according to the allowable stress tables of ASME Section II Part D; above that range a chromium-molybdenum grade such as SA387 is required.
Q: What post-weld heat treatment temperature applies to Gr.70 vessels?
Typically 595 to 650 degrees C for one hour minimum, plus one hour per 25 mm of thickness, with the requirement triggered by thickness and restraint under ASME UCS-56.
Q: Which Chinese grade corresponds to SA516 Gr.70?
Q345R to GB/T 713 covers the same pressure vessel application and similar strength level, but the two are not interchangeable without a design review because chemistry limits, impact requirements and allowable stresses differ.