What S690QL1 Designates Under EN 10025-6
S690QL1 is a quenched and tempered fine-grain structural steel plate defined in EN 10025-6, the part of the European hot-rolled products standard that covers flat products of high yield strength structural steels in the quenched and tempered condition. The designation is a compact contract in itself: S for structural steel, 690 for the minimum specified yield strength in megapascals at the thinnest gauge range, Q for quenching and tempering, L for low-temperature toughness, and the digit 1 for the toughest impact class in that series. A plate ordered as S690QL1 therefore carries a guaranteed minimum yield of 690 MPa together with a minimum Charpy energy of 30 J at -60 degrees Celsius in the longitudinal direction, a combination that separates it from S690Q, S690QL and S690QL2 in everyday procurement.
The practical consequence is that S690QL1 is chosen where a design must shed dead weight without surrendering brittle fracture resistance in a cold climate, a refrigerated service environment or a dynamically loaded structure. Because the specified strength approaches three times that of an ordinary S355 structural plate, the wall thickness of a member can often be reduced by half or more, which lowers self-weight, weld volume and transport cost at the same time. That gain is only realisable if the buyer controls chemistry, heat treatment state and toughness verification as strictly as the strength figure.
Chemical Composition and Carbon Equivalent Limits
EN 10025-6 controls S690QL1 by a table of maximum values rather than a single nominal analysis, which gives the mill freedom to reach the strength and toughness balance through different alloying routes. Carbon is capped at 0.20%, silicon at 0.80%, manganese at 1.70%, phosphorus at 0.020%, sulphur at 0.010% and nitrogen at 0.015%, with boron at 0.005% maximum. The micro-alloying window allows niobium up to 0.06%, vanadium up to 0.12%, titanium up to 0.05% and zirconium up to 0.15%. Strengthening and hardenability elements sit at chromium 1.50%, molybdenum 0.70%, nickel 2.00% and copper 0.50% maximum respectively.
Two consequences follow for the purchaser. First, a plate that meets the table only at its upper limits can be very different in welding behaviour from one that sits near the lower end, even though both are certified as S690QL1. Second, the carbon equivalent value is the controlling number for fabrication. EN 10025-6 limits CEV to 0.83 for thicknesses up to 50 mm and to a slightly higher figure above that, and a mill certificate that reports CEV at 0.80 rather than 0.70 will require a hotter preheat and a tighter heat input window in the fabrication shop. Reading the actual heat analysis on the inspection document, not only the grade stamp, is the first act of competent buying.
Residual element control also matters in this grade because toughness at -60 degrees Celsius is sensitive to sulphur and to inclusion shape. A sulphur level near the 0.010% ceiling, combined with a calcium treatment that is not reported, is a common source of poor through-thickness ductility and lamellar tearing in heavily restrained T-joints. Where the joint design is highly restrained, a Z-quality plate to EN 10164 with a minimum through-thickness reduction of area of 25% or 35% should be specified in addition to the base grade.
Mechanical Properties Across Thickness Ranges
Strength in a quenched and tempered plate falls as section thickness rises, because the centre of a heavy plate cools more slowly during quenching and therefore tempers to a lower strength level. EN 10025-6 handles this by stepping the guaranteed values by thickness band. The figures below reflect the specified minima for S690QL1 and are the values a buyer should compare against the test report before acceptance.
| Nominal thickness (mm) | 3 to 50 | 50 to 100 | 100 to 150 |
|---|---|---|---|
| Minimum yield strength ReH (MPa) | 690 | 650 | 630 |
| Tensile strength Rm (MPa) | 770 to 940 | 760 to 930 | 710 to 900 |
| Minimum elongation A (%, L0 = 5.65 sqrt S0) | 14 | 14 | 14 |
| Minimum Charpy V-notch energy, longitudinal (J) | 30 at -60 C | 30 at -60 C | 30 at -60 C |
| Typical carbon equivalent CEV maximum | 0.83 | 0.85 | 0.85 |
The ratio of tensile to yield strength, roughly 1.10 to 1.36 depending on thickness, is deliberately tight. That narrow band is a quality signature: it shows the plate has been tempered to a uniform structure rather than left with a hard, untempered skin. A tensile result at the top of the range combined with a yield just above the minimum is normal, whereas a yield that overshoots 800 MPa on a 20 mm plate hints at under-tempering and predicts poor toughness in the heat affected zone.
Toughness, Transition Behaviour and Impact Testing
The QL1 suffix is the reason this grade exists in cold-climate projects. Impact testing is carried out on Charpy V-notch specimens taken in the longitudinal direction, and 30 J at -60 degrees Celsius is the floor, not the target. Because the steel is fine grained and fully killed, the ductile-to-brittle transition is steep and sits well below the test temperature, so a result of 100 J or more at -60 degrees Celsius is common on production plates from a controlled rolling and quenching route.
Three verification points deserve attention. Specimen axis and notch location must match the agreed sampling plan; on plates above 40 mm the standard permits testing near the surface or at quarter thickness, and the two locations do not give the same result. The testing temperature tolerance and the soaking time in the cooling bath should be recorded on the certificate, since a nominally compliant test run with a short soak at temperature is not equivalent to a properly stabilised one. Finally, the number of specimens and the retest rules should be agreed before rolling, because a single low value at -60 degrees Celsius can trigger a full re-test batch that delays delivery.
Where the design temperature sits between -40 and -20 degrees Celsius and no dynamic loading is present, S690QL is normally sufficient and cheaper. Choosing QL1 for a mild climate adds cost without technical benefit; choosing QL for an arctic structure is a common and expensive error that only surfaces during third-party inspection.
Quenching and Tempering Route and Heat Treatment Control
Production of S690QL1 follows a disciplined route: primary steelmaking with low sulphur and controlled residuals, secondary refining and vacuum degassing, calcium treatment for inclusion modification, continuous casting into slab, reheating, controlled rolling to a fine austenite grain size, then austenitising, water quenching and tempering. The quench is the step that generates the martensitic and lower bainitic structure; the temper is the step that converts it into a tough tempered martensite with the required strength. Neither step tolerates shortcuts, and the tempering temperature is normally set in the 550 to 650 degrees Celsius region and held long enough for the centre of the heaviest plate in the batch to reach temperature.
Two fabrication rules flow directly from this metallurgy. First, any subsequent thermal cycle above roughly 600 degrees Celsius will soften the plate and reduce the achieved yield strength, so stress relief must be agreed with the mill before the order is placed and the holding temperature, time and cooling rate written into the purchase specification. Second, hot forming is not permitted without a documented re-quench and re-temper, because the original properties are destroyed by the forming temperature. Cold forming is allowed within the radius limits discussed below, and the resulting section will retain its strength provided the outer fibre strain stays modest.
Plates supplied in the as-quenched and tempered condition should not be normalised by the fabricator under any circumstances. Normalising from the delivery condition produces a much lower strength level that cannot be restored without a full reheat treatment, and a normalised S690QL1 plate that is subsequently welded into a structure may still pass a tensile test taken from the parent metal while behaving like a 400 MPa steel in the joint.
Welding S690QL1: Preheat, Heat Input and Consumables
Welding is where most S690QL1 projects succeed or fail. The steel derives its strength partly from a lean alloy design and a very fine microstructure, and the same thermal cycle that produces a sound weld metal can soften the heat affected zone or, at the other extreme, create hard untempered martensite. EN 1011-2 provides the framework for specifying preheat and heat input, and a welding procedure qualification to that framework should precede any production work.
In practice, preheat in the 100 to 150 degrees Celsius range is typical for plate up to 25 mm with a matching strength consumable, rising for thicker sections or higher carbon equivalent values, and a minimum interpass temperature must be maintained rather than allowed to drift downward between passes. Heat input is usually held in a band of roughly 0.8 to 1.5 kJ per millimetre for gas metal arc and submerged arc work, high enough to avoid a hard, crack-sensitive heat affected zone and low enough to avoid over-tempering the parent metal. A run-on and run-off tab prevents the crater and start-stop defects that are disproportionately damaging in a low-toughness-tolerant grade.
Consumables should be hydrogen controlled, handled in heated quivers and used within the manufacturer's stated exposure limits, with a diffusible hydrogen level of H5 or lower for restrained joints. Matching strength consumables are the default for butt welds in thick sections; undermatched consumables are occasionally used for fillet welds or repair welds where dilution control is difficult. Post-weld heat treatment, if required by the design code, must be agreed at the plate order stage because it will reduce the parent metal strength in the same way as any other tempering excursion.
Forming, Cutting and Machining Practice
S690QL1 cold forms well provided the bend radius is generous and the bend line is oriented transverse to the rolling direction where possible. As a working rule for plate up to 20 mm, an inner bend radius of about three to four times the thickness keeps outer fibre strain within a range that experience shows is safe, and heavier plate requires proportionally larger radii. Bending should be done in a single continuous stroke with a machined or rounded punch, and any flame-cut edge within the bend zone should be ground to remove the hardened layer before forming.
Thermal cutting leaves a narrow heat affected zone on any quenched and tempered plate. Laser and plasma cutting produce the cleanest edge; oxy-fuel cutting is acceptable for thicker sections but the cut face should be dressed if it will carry a fatigue load or be welded without a backing strip. The hardened edge layer, typically 0.5 to 2 mm deep depending on process, must be removed by grinding before welding or before any edge that will be subject to impact.
Machining follows conventional rules for a 690 MPa class steel: carbide tooling, positive rake, rigid set-up, generous coolant and lower surface speeds than for mild steel. Drilling benefits from pilot holes and from avoiding work-hardening through dwell. Because the plate is fully tempered rather than case hardened, there is no hard skin to fight, which makes it friendlier on the shop floor than a wear plate of comparable hardness.
Applications and Grade Selection
The dominant uses are mobile and heavy equipment structures where payload and fuel efficiency are commercially decisive: crane booms and jibs, excavator arms and buckets, concrete pump booms, drilling rig masts, and the chassis of haul trucks and loaders. Transport equipment follows the same logic, with weight savings in trailer frames, container handling spreaders and rail vehicle structures. In bridge and building work, S690QL1 appears in heavily loaded truss nodes, arch ribs, temporary works and long-span roof structures where depth is constrained.
Pressure equipment use deserves a caution. A quenched and tempered 690 MPa plate can be used for certain high-pressure vessels and penstock applications, but the applicable pressure vessel code will impose its own allowable stress, impact testing and post-weld heat treatment rules that may override the plate standard. Designers should confirm that the selected code permits this strength class at the intended design temperature, and that weld joint efficiency factors are applied correctly rather than assumed from the parent metal strength.
Selection between S690QL1 and its neighbours is straightforward once service temperature and consequence of failure are known. S690Q for ambient service, S690QL for -40 degrees Celsius, S690QL1 for -60 degrees Celsius, and a step up to S890QL or S960QL only where the weight saving justifies the far tighter welding discipline those grades demand. S690QL1 is usually the practical ceiling for general fabrication yards, because above that level preheat control, consumable handling and non-destructive testing requirements begin to demand specialist capability.
Inspection, Certification and Dimensional Tolerances
An order for S690QL1 should be pinned to EN 10025-6 for the technical delivery conditions, EN 10029 for dimensional and shape tolerances, EN 10160 for ultrasonic testing of the plate interior when specified, and EN 10204 for the inspection document. A 3.1 certificate naming the manufacturer and listing cast number, heat analysis, product analysis, tensile results with thickness and test piece orientation, impact results with test temperature and energy values, and the delivery condition is the minimum acceptable documentation.
Ultrasonic testing class S1 or S2 to EN 10160 is routinely specified for plates above 40 mm used in dynamically loaded structures, and class S2 or S3 where the plate will see through-thickness stress. Visual and dimensional checks should cover thickness at several points rather than a single reading, since a quenched and tempered plate rolled near the lower thickness tolerance can lose a meaningful share of its section, and flatness matters because a distorted plate forces fit-up stresses into the joint. Surface condition should also be examined for grinding marks, rolled-in scale and repair welds, all of which must be documented rather than hidden under paint.
Traceability closes the loop: heat number on the plate edge, heat number on the certificate, and heat number recorded against the piece in the fabrication drawing. For safety-critical structures this is not bureaucracy, it is the only way to answer a question about toughness three years later.
FAQ
Q: What is the difference between S690Q, S690QL and S690QL1?
The letters define the Charpy impact test temperature: S690Q is tested at 0 degrees Celsius, S690QL at -40 degrees Celsius and S690QL1 at -60 degrees Celsius, all at a minimum of 30 J longitudinal. Strength requirements are identical.
Q: What minimum yield strength does S690QL1 guarantee at 60 mm thickness?
At nominal thickness above 50 mm and up to 100 mm, the minimum yield strength is 650 MPa, with tensile strength in the range 760 to 930 MPa. The 690 MPa figure applies only to the 3 to 50 mm band.
Q: Can S690QL1 be welded without preheat?
No. Preheat is required to control cooling rate and hydrogen. A typical range is 100 to 150 degrees Celsius for plate up to 25 mm, increasing with thickness and carbon equivalent, and the exact value should be established by a procedure qualification to EN 1011-2.
Q: Is post-weld heat treatment permissible on this grade?
It can be applied, but any excursion above roughly 600 degrees Celsius reduces the achieved yield strength of the parent metal. The stress relief temperature, hold time and cooling rate must be agreed with the plate manufacturer at the ordering stage and validated by testing of the heat treated condition.
Q: How is S690QL1 verified on delivery?
Check the EN 10204 3.1 certificate against the order: heat analysis and CEV, tensile results with thickness band, Charpy values with test temperature and orientation, and the delivery condition marked as quenched and tempered. For heavy or critical plate, add ultrasonic testing to EN 10160 and confirm flatness and thickness to EN 10029.
Q: Why does a 690 MPa plate sometimes measure lower strength after fabrication?
Because the strength comes from tempering at a controlled temperature. Additional thermal cycles from welding, stress relief or hot forming over-temper the parent metal, and normalising destroys the quenched and tempered structure entirely. Properties can only be restored by a full re-austenitising, quenching and tempering treatment.