P275NH, P275NL1 and P275NL2 are the three low temperature grades of the P275 family in EN 10028-3, the standard for weldable fine grain steels for pressure purposes. They share the same strength level and the same normalised delivery condition, and they differ mainly in how much low temperature impact toughness is guaranteed. Choosing between them is therefore a question of minimum design metal temperature, not of strength.
Reading the Designation
Each element of the designation carries information that has to be respected when the material is ordered.
| Symbol | Meaning |
|---|---|
| P | Steel for pressure purposes |
| 275 | Minimum yield strength of 275 MPa for the thinner thickness classes |
| N | Normalised or normalised rolled delivery condition |
| H | Suitable for elevated temperature service |
| L1 | Low temperature quality, impact tested at minus 40 degrees C |
| L2 | Low temperature quality, impact tested at minus 50 degrees C |
Chemical Composition
All three grades are fine grain steels with a restricted carbon and sulphur content and an aluminium addition to control grain size. The differences between them are concentrated in the residual element limits, which is what allows the L2 quality to hold toughness at the lowest test temperature.
| Element, mass % | P275NH | P275NL1 | P275NL2 |
|---|---|---|---|
| C, max | 0.16 | 0.16 | 0.16 |
| Si, max | 0.40 | 0.40 | 0.40 |
| Mn | 0.80-1.50 | 0.80-1.50 | 0.80-1.50 |
| P, max | 0.025 | 0.025 | 0.020 |
| S, max | 0.015 | 0.015 | 0.010 |
| Cr, max | 0.30 | 0.30 | 0.30 |
| Mo, max | 0.08 | 0.08 | 0.08 |
| Ni, max | 0.50 | 0.50 | 0.50 |
| Nb, max | 0.05 | 0.05 | 0.05 |
| Ti, max | 0.03 | 0.03 | 0.03 |
| V, max | 0.05 | 0.05 | 0.05 |
| N, max | 0.012 | 0.012 | 0.012 |
| Al, min | 0.020 | 0.020 | 0.020 |
| Cu, max | 0.30 | 0.30 | 0.30 |
One additional restriction applies to all three: the combined content of niobium, titanium and vanadium must not exceed 0.05 percent. Micro-alloying is limited deliberately because the grades are intended to be supplied in the normalised condition, where the toughness comes from a refined ferrite grain size rather than from precipitation.
Mechanical Properties
Yield strength is quoted against thickness classes, and the tensile range and elongation requirement are common to the three grades. Verification is by tensile testing of the plate as supplied, with the test direction and specimen location as agreed at ordering.
| Thickness (mm) | Yield strength, min (MPa) | Tensile strength (MPa) | Elongation, min (%) |
|---|---|---|---|
| t <= 16 | 275 | 390-510 | 24 |
| 16 < t <= 40 | 265 | 390-510 | 24 |
| 40 < t <= 60 | 255 | 390-510 | 24 |
| 60 < t <= 100 | 245 | 390-510 | 23 |
| 100 < t <= 150 | 235 | 390-510 | 23 |
| 150 < t <= 250 | 225 | 390-510 | 23 |
The Real Difference: Impact Toughness
This is the only property that separates the three grades in normal engineering use, and it drives the minimum design metal temperature that the vessel or exchanger can be built to.
| Grade | Impact test temperature (C) | Minimum absorbed energy | Typical service |
|---|---|---|---|
| P275NH | +20 | 40 J | Boilers and vessels at moderate to elevated temperature |
| P275NL1 | -40 | 27 J | Low temperature service, cold climates |
| P275NL2 | -50 | 27 J | Especially low temperature service |
The H suffix on the first grade also signals suitability for elevated temperature service, which is why P275NH appears in boiler and heat exchanger work where the metal temperature is above ambient but where low temperature toughness is not a design driver. If a specification calls for both elevated temperature strength and low temperature toughness, that combination has to be addressed explicitly, because the designations cover the two duties in different ways.
Fabrication and Heat Treatment
All three grades are welded by the conventional arc processes with low hydrogen consumables, and the aluminium addition that makes them fine grained also helps keep the heat affected zone tough. Because the property that the L1 and L2 qualities pay for is toughness, any thermal operation after delivery must be controlled: hot forming above the tempering range, or post-weld heat treatment at excessive temperature, can coarsen the grain structure and destroy the impact energy that was tested at the mill. Where such treatment is unavoidable, the impact properties are normally re-verified on a test piece that has seen the same thermal cycle as the component. Plate is supplied in the normalised condition, and re-normalising by a fabricator requires a procedure agreed with the purchaser because it changes the delivery condition of the material.
Applications
P275NH, P275NL1 and P275NL2 are used for pressure vessels, industrial boilers, heat exchangers, compressed gas and chemical storage, compressor casings and pressurised piping systems. The grades are attractive to fabricators because they combine predictable strength with low carbon equivalents, which keeps welding procedures simple, and because they are widely stocked, so plate can be supplied quickly from stock rather than waiting for a special rolling programme.
Frequently Asked Questions
Q: What is the difference between P275NH, P275NL1 and P275NL2?
A: The impact test temperature and the residual element limits. P275NH is tested at plus 20 degrees C with a 40 J minimum, P275NL1 at minus 40 degrees C and P275NL2 at minus 50 degrees C, both with a 27 J minimum.
Q: What does the N in P275NH stand for?
A: Normalised or normalised rolled delivery condition, which refines the ferrite grain size and gives the toughness and consistency the grade is bought for.
Q: What is the minimum yield strength?
A: 275 MPa for plate up to 16 mm thick, falling progressively to 225 MPa for plate between 150 mm and 250 mm thick.
Q: Is there a limit on micro-alloying additions?
A: Yes. The combined niobium, titanium and vanadium content may not exceed 0.05 percent, and aluminium must be present at a minimum of 0.020 percent so that the steel is fully fine grained.
Q: Can the plates be heat treated after delivery?
A: They can, but any operation above the normal tempering range risks coarsening the grain structure and losing the guaranteed impact energy, so the thermal cycle has to be agreed and normally re-verified by testing.
Q: What is the tensile strength range?
A: 390 to 510 MPa across all thickness classes for all three grades, with minimum elongation of 24 percent for thinner plate and 23 percent for heavy plate.