What Stainless Steel Sheet Actually Is
Stainless steel sheet is a flat-rolled steel product whose thickness is small relative to its width, made from an iron-base alloy carrying at least 10.5% chromium by mass. The chromium oxidises at the surface and forms a passive film only a few nanometres thick; that film, not the bulk analysis, decides whether a component survives ten years in a dairy plant or two seasons on a coastal roof. Trade writing often splits the family into "stainless steel", meaning resistance to steam, water and atmospheric moisture, and "acid-resistant steel", meaning resistance to acid, alkali and salt media. Metallurgically they are one product group, and the practical distinction is simply how much chromium, molybdenum and nickel the heat contains and what corrosion test evidence accompanies it.
Thickness conventions matter at the point of order. Under ASTM A480 the dividing line between sheet and plate is 4.76 mm (3/16 in): material thinner than that is sheet, heavier material is plate. Chinese practice uses 3.0 mm as the usual break, with cold-rolled sheet specified under GB/T 3280 and hot-rolled sheet plus plate under GB/T 4237. European buyers work from EN 10088-2, which covers hot-rolled and cold-rolled sheet, plate and strip of corrosion-resistant steels in one document, and Japanese mills quote JIS G 4304 for hot-rolled and JIS G 4305 for cold-rolled material. Grade designations differ between systems even when the alloy is identical: 304 is 06Cr19Ni10 in GB/T 20878, SUS304 in JIS, 1.4301 in EN, and S30400 in UNS. A purchase order that names only one designation invites substitution, so cross-reference at least two systems in the technical annex.
The Four Metallurgical Families and What Separates Them
Sheet grades are grouped by crystal structure, because structure controls strength, magnetism, weldability and the temperature window in which the material can work. Austenitic grades are face-centred cubic, non-magnetic in the annealed condition, and harden only by cold work; they dominate because they combine ductility with weldability. Ferritic grades are body-centred cubic, magnetic, cheaper because they carry little or no nickel, and less ductile in the through-thickness direction. Martensitic grades are hardenable by quenching and tempering and are used where wear or a cutting edge is required rather than corrosion resistance. Duplex grades mix austenite and ferrite roughly 50/50, giving roughly twice the yield strength of 304 with markedly better chloride resistance. Precipitation-hardening grades sit inside the martensitic and semi-austenitic space and reach very high strength after a solution and ageing cycle.
One number summarises chloride resistance better than any marketing claim: the pitting resistance equivalent number, PREN = %Cr + 3.3 x %Mo + 16 x %N. A 304 heat typically calculates to about 18-20, 316L to 25-28 and a 22Cr duplex to 34-36. Field failures in coastal or chloride-bearing service are usually explained by a PREN that was too low for the chloride level and the temperature, not by a defective heat.
| Family | Representative grade | Structure | Typical PREN | Magnetic | Where it is the right choice |
|---|---|---|---|---|---|
| Austenitic | 304 / 304L, 316L | Fully austenitic | 18-28 | No | Food, architectural, general process plant, deep-drawn parts |
| Austenitic, stabilised | 321, 347 | Fully austenitic | 18-20 | No | Service in the 425-815 degrees C sensitisation band, welded vessels |
| Ferritic | 430, 409, 410S | Ferritic | 11-18 | Yes | Appliance panels, exhausts, cookware bases, non-chloride indoor work |
| Martensitic | 410, 420, 431 | Martensitic after quench | 12-16 | Yes | Cutlery blades, wear strips, shafts, tempered structural parts |
| Duplex | 2205 (S32205), 2304 | Austenite plus ferrite | 26-36 | Slightly | Desalination, pulp digesters, marine structures, storage tanks |
| Precipitation hardening | 630 (17-4PH, S17400) | Martensitic after ageing | 15-17 | Yes | High-strength valves, pump shafts, aerospace fittings |
Grade Chemistry: What the Certificate Should Show
Composition limits are the first line of acceptance. The table below lists the ranges that appear in ASTM A240/A240M and in GB/T 20878 for the grades most often ordered as sheet. Note where the "L" version differs: the low-carbon variant restricts carbon to 0.030% so that chromium carbides do not precipitate at grain boundaries during welding, which is the mechanism behind sensitisation and intergranular corrosion. Where a heat will be welded into a heavy section and cannot be solution annealed afterwards, order the L grade rather than testing the standard grade's luck.
| Grade | C max % | Cr % | Ni % | Mo % | Other |
|---|---|---|---|---|---|
| 304 | 0.07 | 18.0-20.0 | 8.0-10.5 | - | Mn 2.00 max, Si 0.75 max |
| 304L | 0.030 | 18.0-20.0 | 8.0-12.0 | - | Mn 2.00 max |
| 316L | 0.030 | 16.0-18.0 | 10.0-14.0 | 2.00-3.00 | N 0.10 max |
| 321 | 0.08 | 17.0-19.0 | 9.0-12.0 | - | Ti 5 x C to 0.70 |
| 430 | 0.12 | 16.0-18.0 | 0.75 max | - | Mn 1.00 max |
| 410S | 0.08 | 11.5-13.5 | 0.60 max | - | Ti or Nb stabilised variants common |
| 2205 (S32205) | 0.030 | 22.0-23.0 | 4.5-6.5 | 3.0-3.5 | N 0.14-0.20 |
| 309S | 0.08 | 22.0-24.0 | 12.0-15.0 | - | High-temperature service |
| 310S | 0.08 | 24.0-26.0 | 19.0-22.0 | - | Furnace and kiln work |
Residual elements deserve a line in the specification as well. Copper above roughly 0.50% raises hot-cracking risk in austenitic welds; sulphur above 0.010% degrades weld penetration and, in duplex grades, shifts the austenite-ferrite balance; and a nitrogen range rather than a maximum is essential for duplex, because nitrogen is doing real strengthening work there. Ask for the actual heat analysis, not just conformance to a maximum, whenever the sheet will be welded under restraint.
Mechanical and Physical Properties That Drive Design
Annealed austenitic sheet is specified by minimum proof and tensile values, and designers should treat those minima as floor values achievable in every heat rather than as expected averages. For 304 sheet in the annealed condition ASTM A240 requires 205 MPa minimum 0.2% proof stress, 515 MPa minimum tensile strength and 40% elongation in 50 mm; 316L requires 170 MPa, 485 MPa and 40%; 430 requires 205 MPa, 450 MPa and 22%; and 2205 duplex requires 450 MPa, 620 MPa and 25%. The gap between 304 and duplex yield strength, roughly 205 against 450 MPa, is the single strongest argument for duplex in tank shells where thickness is governed by strength rather than corrosion allowance.
Physical data matter for thermal design. Austenitic sheet has a density near 7.9-8.0 g/cm3, a modulus around 193-200 GPa at room temperature and a coefficient of thermal expansion close to 17 x 10-6 per K over 0-100 degrees C, which is roughly 1.5 times that of carbon steel and the reason stainless exchangers and ducting need more expansion freedom than the mild-steel drawings suggest. Ferritic 430 expands at about 10 x 10-6 per K and is the better choice where differential expansion against a carbon steel frame would otherwise load the welds. Thermal conductivity of austenitic sheet is low, about 16 W/m.K at room temperature against roughly 45 W/m.K for carbon steel, so heat-tinted welds cool slowly and distortion control becomes a welding-sequence problem rather than a current-setting problem.
Cold work changes these numbers quickly. A 304 sheet rolled to a 1/2 hard temper can exceed 900 MPa tensile, but elongation falls and the material becomes mildly magnetic because some austenite transforms to martensite. If a drawing calls for non-magnetic behaviour after severe forming, specify the annealed temper and design the forming operation around it rather than accepting a magnetic finished part.
Surface Finishes and How They Are Verified
Finish is a specification in its own right and the most common source of disputes on stainless sheet, because a finish name describes a process route rather than a measurable surface. No.1 is hot rolled, annealed and descaled, with a rough, matte appearance and a thickness range that starts around 3 mm. 2D is cold rolled, annealed, pickled and descaled, matte and suitable for further polishing or for painted and lined equipment. 2B is cold rolled, annealed and skin passed, the default for most industrial and architectural work, typically with a roughness Ra of about 0.1-0.5 micrometres and a mildly reflective grey appearance. BA is bright annealed in a controlled atmosphere without pickling, giving a highly reflective finish with Ra often below 0.1 micrometre, and it is the finish to specify where no further polishing is possible. No.4 is a polished finish produced with abrasives of about 120-150 grit, with Ra typically 0.4-1.0 micrometre and visible short directional lines; hairline is a finer, longer, unidirectional pattern; No.8 is a mirror polish achieved by progressive abrasion and buffing.
Verify finish with a roughness instrument rather than by eye, and agree the measurement direction in the technical annex, because Ra read across the polishing lines is routinely two to three times the value read along them. Gloss units are a poor substitute on their own: a 2B surface can read high gloss under diffused light and still fail a weld-cleanliness requirement. On sheet that will be laser cut and left visible, also agree which face is the display face and how protective film is to be applied, since film adhesive left in sun for months leaves residue that needs solvent removal and can stain a BA surface.
Thickness, Width, Flatness and Weight Tolerances
Thickness tolerance is where money is made and lost. Cold-rolled sheet tolerances are fixed by GB/T 708, hot-rolled by GB/T 709, and both ASTM A480 and EN 10088-2 set their own tables; a mill may legitimately ship the minus side of the permitted band, so a 1.0 mm nominal sheet can be supplied close to 0.91 mm under a normal tolerance and about half that deviation under a restricted tolerance. Order restricted tolerance, sometimes called half-normal, whenever the sheet will be formed or the weight of a finished part is contractual. Measure with a micrometre at several points and at least 20 mm in from the edges, and record crown, which is the systematic thickening at the centre of the strip.
Width and length tolerances, squareness, camber and flatness are separate line items. Camber is quoted as the maximum deviation from a straight edge over a stated length; flatness is quoted as the maximum gap under a straightedge, and for laser-cut blanks it is flatness, not thickness, that decides whether the part sits down on the bed. Theoretical weight follows directly: mass in kg per square metre equals thickness in millimetres multiplied by density, so 1.0 mm of 304 at 7.93 g/cm3 gives 7.93 kg/m2, the same thickness in 316L at 7.98 g/cm3 gives 7.98 kg/m2, and in 430 at 7.70 g/cm3 gives 7.70 kg/m2. Comparing actual weighed mass against the theoretical figure computed from measured thickness is a fast check on whether the delivered sheet matches the certified gauge.
Forming, Welding and Post-Weld Treatment
Austenitic sheet work-hardens rapidly, so forming should be planned as a sequence of light passes with intermediate annealing rather than one heavy draw. Springback is large, roughly double that of mild steel at the same tooling geometry, and the material's low thermal conductivity keeps heat in the deformation zone. Use bending radii of at least one thickness for 304 in the soft temper, more for the 316 grades and for hard tempers. Ferritic 430 needs larger radii relative to thickness and is sensitive to grain coarsening if annealed too hot, which shows up as orange-peel on formed surfaces.
For welding, 304 and 304L are joined with ER308L filler, 316L with ER316L, 321 with ER347, 310S with ER310, and duplex 2205 with a matching 22Cr filler that carries extra nickel to balance the ferrite. Austenitic sheet needs no preheat; keep interpass temperature below about 150 degrees C, use low heat input with stringer beads rather than weaves, and purge the root with argon when the back face must remain corrosion resistant. Do not use copper backing bars in contact with the weld pool. After welding, restore the passive film by pickling with a nitric-hydrofluoric acid gel followed by passivation; ASTM A380 covers cleaning and descaling, and ASTM A967 covers chemical passivation tests. Free iron contamination from carbon steel tooling, wire brushes or grinding discs is the most common cause of localised rust on a new stainless installation, so keep dedicated stainless tools and separate storage.
Heat tint is more than cosmetic. The oxide colours that form on a weld correspond to a chromium-depleted zone underneath, and a straw-to-blue tint can lower pitting resistance in that band well below the parent metal. On sanitary and marine work, remove tint completely rather than hoping a wash will do.
Applications, Acceptance and Common Misunderstandings
Typical end uses separate cleanly by grade. 304 and 304L sheet serve food processing, brewing tanks, kitchen equipment, architectural cladding, handrails, ducting and general fabrication. 316L adds molybdenum and goes into pharmaceutical clean rooms, marine fittings, pulp and paper, chemical tanks and coastal architecture. 430 covers appliance panels, cookware and indoor trim where the environment is dry. 2205 duplex covers desalination trains, tanker structures, digesters and chloride-bearing process piping. 309S and 310S sheet belong to furnace and kiln work, covered separately by the oxidation and creep limits of high-temperature grades.
Acceptance documentation should include a mill test certificate to EN 10204 3.1 tied to the heat number stamped or printed on the sheet, the applicable product standard and grade, the actual heat analysis, tensile results, and intergranular corrosion testing such as ASTM A262 Practice E for austenitic grades or ASTM A923 for duplex. Check that the certificate grade matches the ordered designation in both the UNS and EN systems, check the surface finish code, and check the dimensions against the tolerance table you ordered under. A certificate that quotes an ASTM product standard but a GB grade name is not wrong, but it needs an explicit cross-reference note.
Three misunderstandings account for most field complaints. The first is that stainless steel does not corrode: it does, particularly in crevices, under deposits and where chlorides concentrate during evaporation, and no grade resists warm chloride stress corrosion cracking indefinitely. The second is that a magnet proves the grade: cold-worked 304 is magnetic and 316 can be slightly magnetic after drawing, while a fully ferritic 430 is reliably magnetic in every condition. The third is that higher hardness means better wear: austenitic sheet work-hardens but has poor resistance to sliding wear and galling, which is best handled by a different alloy or a surface treatment rather than a harder temper.
FAQ
Q: What is the difference between 304 and 304L sheet?
Both carry 18.0-20.0% chromium and 8.0% or more nickel, but 304 permits up to 0.07% carbon while 304L is limited to 0.030%. The lower carbon prevents chromium carbide precipitation in the 450-850 degrees C range, so 304L keeps its intergranular corrosion resistance after welding without a post-weld solution anneal.
Q: Which finish should be ordered for a sheet that will be visible and unpainted?
2B is the standard industrial finish and is acceptable for many visible indoor panels, but No.4 polished or hairline is normally specified where scratches and fingerprints must be tolerated. BA is chosen when no polishing is possible after fabrication and a bright reflective surface is required.
Q: How much does 1 mm stainless steel sheet weigh per square metre?
Mass equals thickness in millimetres times density, so 1 mm of 304 at 7.93 g/cm3 is 7.93 kg/m2, 1 mm of 316L at 7.98 g/cm3 is 7.98 kg/m2, and 1 mm of 430 at 7.70 g/cm3 is 7.70 kg/m2. Weighing delivered sheet against this figure is a quick gauge check.
Q: Can 304 sheet be used outdoors near the sea?
It can, but tea-staining and pitting are likely within a few kilometres of breaking surf, and crevices at fixings are the first failure points. 316L is the usual minimum for coastal exteriors, and in heavy chloride splash zones a higher-molybdenum or duplex grade is more economical than repeated cleaning.
Q: Why did my stainless sheet rust after welding?
Free iron contamination from carbon steel brushes, files or grinding discs, combined with heat tint that was not removed, leaves a chromium-depleted surface that rusts in days. Pickle and passivate the weld zone, and keep stainless fabrication tools separate from carbon steel tools.
Q: Does 2205 duplex sheet replace 316L one for one?
Not directly. Duplex offers about twice the yield strength and far better chloride resistance, but it is limited to a service temperature below roughly 300 degrees C because of embrittlement above that range, needs a controlled welding procedure with balanced ferrite, and is less tolerant of heavy cold forming than 304L.