What 20Cr Actually Is
20Cr is a low-carbon, chromium-bearing carburising steel listed in GB/T 3077, the Chinese standard for alloy structural steel. The designation follows the usual convention: the leading figure is the nominal carbon content in hundredths of a percent, so 20Cr carries about 0.20 percent carbon, and the suffix identifies chromium as the only deliberate alloying addition, at roughly 1 percent. It is a case-hardening grade, not a through-hardening grade: the low carbon core stays tough and shock resistant, while the surface is enriched in carbon and hardened to carry contact stress and wear.
Confusion around the grade is common because the same symbol appears in three different commercial contexts. To a machinist running automatic lathes it is bar stock, often cold drawn or ground, chosen for consistent machinability. To a heat treater it is a carburising job with a specified case depth and a specified core hardness. To a designer it is a compromise grade, sitting between plain carbon case-hardening steel and the higher-hardenability manganese-chromium grades, and it is chosen precisely when the section is small enough that a modest hardenability is sufficient.
Chemical Composition and Grade Control
The composition window is narrow by design, because carbon and chromium together set both the case response and the core toughness. Chromium raises hardenability and forms wear-resistant carbides in the case, but excess chromium in a 0.20 percent carbon steel promotes retained austenite after carburising and makes case depth control less predictable.
| Element | Typical range (wt. %) | Function |
|---|---|---|
| C | 0.18-0.24 | Sets core strength; the low base leaves room for carburising |
| Si | 0.17-0.37 | Deoxidation; excess raises tempering resistance and scale |
| Mn | 0.50-0.80 | Hardenability and deoxidation; too high embrittles the case |
| Cr | 0.70-1.00 | Hardenability, case wear resistance, carbide formation |
| P | 0.035 max | Residual; raises temper embrittlement risk |
| S | 0.035 max | Residual; free-machining variants trade toughness for it |
| Cu, Ni | 0.30 max each | Residuals from scrap; controlled to protect forgeability |
Two order details decide whether the delivered bar behaves as expected. The first is hardenability control: GB/T 3077 controls chemistry, not the position of the hardness curve, so a buyer who needs repeatable case and core hardness after heat treatment should specify a hardenability-guaranteed grade per GB/T 5216 with a stated end-quench limit. The second is deoxidation and grain size: 20Cr is prone to grain coarsening during a long carburising hold, and a fine-grain, aluminium-killed heat with a stated prior austenite grain size is far easier to control than a rimmed or coarse-grain alternative. Cold-drawn and ground bar for turned parts is normally ordered to GB/T 3078, while hot-rolled bar dimensions follow GB/T 702.
Mechanical Properties and Hardenability
In the quenched and tempered condition the grade delivers moderate strength with good ductility, which is the whole point of a carburising steel: the core must bend rather than snap. Properties commonly quoted for small sections in the quenched and tempered state are a tensile strength of about 835 MPa minimum, a yield strength of about 540 MPa minimum, elongation around 10 percent, reduction of area around 40 percent and impact energy around 47 J, with the exact figures taken from the applicable standard table for the delivered size and condition.
Hardenability is the limiting property. The critical diameter for a fully martensitic core is roughly 4 to 22 mm in oil and roughly 11 to 40 mm in water, depending on austenitising temperature, grain size and the severity of agitation. The end-quench curve is correspondingly shallow, and a half-martensitic hardness is reached at about 20 to 23 mm from the quenched end. The practical meaning is blunt: 20Cr works in pins, bushes, small gears, spindles and thin-walled components, and it does not work in a 60 mm shaft that must be hard right through. Where the section is thicker, a manganese-chromium grade or a molybdenum-bearing grade is the correct answer, not a longer quench.
| Grade | C (%) | Cr (%) | Other | Behaviour | Typical use |
|---|---|---|---|---|---|
| 15Cr | 0.12-0.18 | 0.70-1.00 | - | Softer core, better toughness, lower case support | Thin-section bushes, lightly loaded pins |
| 20Cr | 0.18-0.24 | 0.70-1.00 | - | Balanced core strength and toughness | Small gears, shafts, wear pins, cold-work moulds |
| 20CrMo | 0.17-0.24 | 0.85-1.25 | Mo 0.15-0.25 | Higher hardenability, better temper resistance | Larger carburised gears |
| 20CrMnTi | 0.17-0.23 | 1.00-1.30 | Mn 0.80-1.10, Ti | Fine grain, direct quenching possible | Automotive gears and shafts |
Carburising and Case Hardening
The grade is designed for a carburised case of roughly 0.6 to 1.0 percent carbon in the surface layer, produced at 900 to 930 degree C in a gas atmosphere, followed by quenching and low-temperature tempering. Effective case depth is measured and verified per GB/T 9450, and it should be specified as a depth to a defined hardness limit, not as "deep case", because the two numbers are not interchangeable and the case depth must be matched to the tooth or contact geometry.
Case hardness of 58 to 62 HRC, measured per GB/T 230.1, is the normal target for a carburised and quenched surface, giving fine acicular tempered martensite. The core becomes low-carbon lath martensite with a hardness of about 30 to 40 HRC, which supplies the strength to support the hard case without transmitting shock into a brittle substrate. This combination of a hard surface over a tough core is why the grade is used for components loaded in both wear and impact, such as chain pins, cam followers, guide bushes and the cavities of cold-work moulds.
One characteristic of 20Cr must be respected in the process route: the steel has a tendency to grain growth during a prolonged carburising hold. If the part is cooled directly from the carburising temperature and quenched, the coarse prior austenite grain size reduces impact toughness in the core. The conventional remedy is a secondary quench: after carburising, the part is cooled, re-austenitised at a lower temperature such as 860 to 880 degree C so that the grain structure is refined, and then quenched and tempered. A fine-grain, aluminium-killed heat with titanium or niobium micro-addition reduces the problem, which is exactly why 20CrMnTi is preferred for large automotive gears.
Heat Treatment Practice Beyond Carburising
Normalising is used both as a pre-machining treatment and as a structure conditioner. It refines the coarse proeutectoid ferrite, breaks up banding and prepares the structure for spheroidisation, and it produces a hardness in the 170 to 217 HB range in which the relative machinability is about 65 percent of a free-cutting reference.
Annealing is the treatment to avoid before machining. A fully annealed 20Cr is soft and gummy, and the built-up edge that forms on the tool produces poor surface finish and short tool life. Where an annealed structure is unavoidable for forming, the part should be normalised or hardened and tempered before the finishing cut, and the finishing operation should be scheduled after the last heat treatment that changes dimensions.
Quenching and tempering is performed at about 860 to 880 degree C in oil, followed by tempering at 150 to 200 degree C for components where surface hardness matters, or at a higher temperature where core toughness dominates. Tempering in the 250 to 400 degree C range should be avoided because it produces the lowest toughness for a given strength, the classic temper embrittlement window. The grade shows no pronounced temper brittleness provided phosphorus and residual elements are controlled, and it retains good low-temperature impact toughness after quenching and low-temperature tempering, which suits parts that see winter service.
Machining, Welding and Forming Characteristics
Machinability is good in the normalised or quenched-and-tempered condition and poor after annealing, a distinction that directly affects the process routing for turned parts. The grade has high cold-strain plasticity and can be drawn cold, which is why cold-drawn and ground bar is a standard supply form for small precision components and why the dimensional consistency of cold-drawn stock is often worth more than the small price difference against hot-rolled bar.
Weldability is moderate. The low carbon content keeps the heat-affected zone from hardening severely, and post-weld heat treatment is generally not required for thin sections. Where the part is thicker than about 15 mm, preheating to 100 to 150 degree C before welding is standard practice to slow the cooling rate and avoid hydrogen-assisted cracking, and parts that are subsequently carburised should have weld spatter and oxide removed before the case-hardening operation.
Supply Forms, Applications and Selection Rules
20Cr is stocked as hot-rolled round bar, cold-drawn bar, peeled and ground bar, hot-rolled plate, cold-rolled sheet and coil, and seamless tube, in diameters and thicknesses that match the small-section duty the grade is designed for. For turned hardware components the usual choice is cold-drawn bar in the normalised or tempered condition, cut to length and finished without further structural heat treatment.
Applications cluster where a hard, wear-resistant skin and a shock-tolerant core are needed in a section that a 1 percent chromium addition can harden: gear teeth in small reducers, shafts and spindles, chain pins and bushings, guide pins and wear plates in fixtures, cam rollers and the cavities of cold-working moulds. In mould service the cavity is machined, carburised, quenched and low-temperature tempered to give a surface of 58 to 62 HRC with a tough backing; for short-production moulds where wear is not the governing failure mode, a direct quench and temper without carburising is an acceptable and cheaper route.
Selection should be driven by section size first, then by the required case depth, then by core toughness. If the finished section exceeds roughly 25 mm at the point of maximum stress, the hardenability of 20Cr becomes the limitation and a molybdenum or manganese-chromium grade should be evaluated on the end-quench curve rather than on price. If the part will be welded after carburising, the sequence is wrong by definition and must be re-planned. If the required core strength exceeds about 1000 MPa, the carbon level is too low and a medium-carbon alloy steel, not a deeper case, is the answer.
Inspection and Acceptance Points
Acceptance should be written around the properties that control performance, not around a certificate headline. Chemical composition is verified against GB/T 3077, with the certificate stating the actual heat analysis and the product analysis. Hardenability-critical orders should require the end-quench curve or the guaranteed hardness limits per GB/T 5216, measured on the actual heat. Non-metallic inclusion content per GB/T 10561 and prior austenite grain size per GB/T 6394 are the two metallurgical checks that predict whether the carburising response will be repeatable.
For the finished part, effective case depth per GB/T 9450, surface hardness per GB/T 230.1, core hardness and a metallographic assessment of the case structure, including retained austenite and any carbide network, form a complete release package. Decarburisation on the bar surface should be checked because a decarburised layer carburises differently and produces soft spots on finished teeth. Surface defects such as seams and laps must be removed before carburising, since a seam becomes an oxide-filled crack after quenching and becomes a fatigue origin in service.
FAQ
Q: What does the 20 in 20Cr mean?
The 20 denotes a nominal carbon content of about 0.20 percent and the Cr denotes chromium at roughly 1 percent; the grade is defined in GB/T 3077 as a chromium alloy structural steel for carburising.
Q: Is 20Cr the same as 20CrMnTi?
No. 20CrMnTi adds manganese and titanium, which raise hardenability and refine the grain, so it tolerates direct quenching after carburising; 20Cr generally needs a secondary quench to recover core toughness.
Q: Can 20Cr be through hardened in a 50 mm section?
Not reliably. Its critical diameter is roughly 4 to 22 mm in oil and roughly 11 to 40 mm in water, so a 50 mm section will not develop a fully martensitic core; a higher-hardenability grade should be selected.
Q: Why does 20Cr machine badly after annealing?
A fully annealed structure is soft and produces a built-up edge, giving poor finish and short tool life; normalising to about 170 to 217 HB or quenching and tempering restores machinability to roughly 65 percent of a free-cutting reference.
Q: What case hardness is expected after carburising and quenching?
A surface of 58 to 62 HRC in the form of fine acicular tempered martensite, over a core of low-carbon martensite at about 30 to 40 HRC, is the normal target for this grade.
Q: Is preheating required before welding 20Cr?
For sections thicker than about 15 mm, preheat to 100 to 150 degree C is standard practice; thin sections with this carbon level usually weld without preheat and without post-weld heat treatment.