What SA387 Grade 22 Class 2 Plate Is

ASTM A387/A387M covers chromium-molybdenum alloy steel plates intended for welded boilers and pressure vessels that operate at elevated temperature. Grade 22 is the 2.25% Cr – 1% Mo family, and Class 2 denotes plate supplied in the normalized and tempered condition with a higher minimum tensile strength than Class 1, which is normally supplied annealed. The same material is published in the ASME Boiler and Pressure Vessel Code as SA-387 Grade 22 Class 2, so a plate ordered to either designation is accepted for Code construction when the certificate, heat treatment and impact data line up with Section II Part A.

The reason the grade exists is creep strength combined with hydrogen resistance. Plain carbon steel loses useful strength above roughly 400 °C, whereas 2.25Cr-1Mo holds design strength through the 450–580 °C band and, just as importantly, resists high-temperature hydrogen attack. That is why hydroprocessing reactors, coke drums, hot high-pressure separators and heavy-wall heat exchanger shells are still built from this grade rather than from carbon steel or from the 1.25Cr family.

Class 2 is not simply "stronger plate". The higher strength comes from normalizing followed by tempering, which produces a tempered bainite microstructure. That structure is tougher than the annealed ferrite-pearlite of Class 1 at the same chromium level, but it is also more sensitive to welding variables and to post-weld heat treatment discipline, so the two classes should not be treated as interchangeable in a fabrication procedure.

Chemical Composition and Product Analysis Limits

Grade 22 chemistry is tight enough that the balance between chromium and molybdenum determines both hardenability and the resistance to temper embrittlement. Two sets of limits matter to a purchaser: the ladle analysis limits of the product specification, and the slightly wider product-analysis tolerances that apply when a sample is taken from the finished plate. A mill certificate that reports only the ladle figures leaves the buyer unable to confirm that the plate itself is inside the permissible drift.

Element Ladle analysis, % Product analysis, % Why it matters
C 0.05–0.15 0.04–0.15 Strength and hardenability; high carbon hurts toughness in the heat-affected zone
Si 0.50 max 0.55 max Deoxidation; excess silicon promotes temper embrittlement
Mn 0.30–0.60 0.25–0.66 Hardenability and sulphur control
P 0.035 max 0.035 max Segregation and temper embrittlement; lower is always better in thick plate
S 0.035 max 0.035 max Inclusion content, through-thickness ductility, lamellar tearing risk
Cr 2.00–2.50 1.88–2.62 Creep strength and oxidation resistance
Mo 0.90–1.10 0.85–1.15 Creep rupture strength and resistance to hydrogen attack

For hydrogen service the residual elements that are not in the table often decide the outcome. Copper, tin, antimony and arsenic are not specified in the base grade, but they concentrate in the grain boundaries during tempering and raise the ductile-to-brittle transition temperature of the heat-affected zone. Buyers specifying plate for hydrotreaters routinely add a restriction on the sum of these residuals, together with a maximum phosphorus well below the 0.035% default, and ask for the values to be reported per heat rather than as a generic statement.

Mechanical Properties: Class 1 versus Class 2

Tensile testing is performed on specimens taken transverse to the rolling direction unless the order states otherwise, and the acceptance figures below are the specification minima, not typical mill results. A mill that consistently ships at the minimum has no margin for the strength loss that occurs after post-weld heat treatment, which is why experienced buyers review the actual values rather than the compliance statement.

Property Grade 22 Class 1 (annealed) Grade 22 Class 2 (normalized and tempered)
Tensile strength 415–585 MPa 515–690 MPa
Yield strength, 0.2% offset 220 MPa min 310 MPa min
Elongation in 50 mm 18% min 18% min
Typical delivery condition Annealed Normalized and tempered
Typical application temperature Moderate wall, moderate temperature Heavy wall, 450–580 °C design

Impact testing is not mandatory in the base grade for all thicknesses, but it becomes effectively mandatory in cold-climate projects, in thick sections and wherever the purchase order invokes a supplementary requirement. When impact data are required, confirm the test temperature, the specimen size, the acceptance energy and whether the tests are taken after simulated post-weld heat treatment. A Charpy value measured on as-normalized plate says very little about the same plate after twenty hours at 690 °C.

Heat Treatment, Microstructure and Temper Embrittlement

Grade 22 Class 2 is normalized in the region of 900–955 °C, then tempered. The tempering temperature is the single most important number on the route card, because it sets the balance between strength and toughness and because it must be at or above the minimum required by the specification for Class 2 plate. Purchasers should read the actual tempering temperature and holding time on the certificate instead of accepting the words "normalized and tempered" as sufficient evidence.

Temper embrittlement is the characteristic risk of this grade. Holding 2.25Cr-1Mo in the 375–575 °C range, or cooling slowly through it, allows phosphorus and trace tramp elements to segregate to prior austenite grain boundaries; the room-temperature toughness falls while tensile strength is unaffected, so the problem is invisible in a standard tensile test. Two controls are used in practice. The first is metallurgical: low phosphorus, low silicon, restricted residuals. The second is procedural: fast cooling after tempering and after post-weld heat treatment, and a step-cooling test to demonstrate that the heat in question has margin.

Step cooling is a defined thermal cycle that accelerates the segregation that would otherwise take years in service, after which Charpy specimens are tested and the shift in transition temperature is measured. Where the purchase order invokes this evaluation, agree in advance on the starting condition of the specimens, the number of tests, and the acceptance shift, and require the results to be reported per heat treatment lot rather than per heat only.

Welding, Preheat and Post-Weld Heat Treatment

The grade is readily weldable but not forgiving. Preheat in the 200–250 °C range is standard for wall thicknesses above about 25 mm, and the interpass temperature is normally capped near 300 °C to keep the heat-affected zone from coarsening. Matching consumables are the 2.25Cr-1Mo classification, for example covered electrodes to AWS A5.5 E9018-B3 or solid wire to AWS A5.28 ER90S-B3; the B3 suffix identifies the deposited chemistry, and substituting a 1.25Cr consumable changes the creep behaviour of the joint.

Post-weld heat treatment is required for essentially all Code construction in this grade. The hold is normally placed in the 690–710 °C window for heavy sections, with a controlled heating and cooling rate above 400 °C; the exact parameters belong in the qualified welding procedure and must be consistent with the tempering temperature used by the mill, otherwise the weld zone and the parent plate finish at different strength levels. Thermocouple placement, number of heats treated together, and the recording of the actual chart are all legitimate items for a third-party witness to check.

Practical shop points that repeatedly cause trouble: flame-cut edges must be ground back far enough to remove the hardened layer before welding; temporary attachments leave weld metal that has to be removed rather than blended; repair welds need their own procedure qualification and their own heat treatment record. Hydrogen cracking in this grade usually originates at a weld toe that cooled too fast after a repair, not in the production seam.

Plate Dimensions, Tolerances and Non-Destructive Testing

Thickness tolerance is governed by the general requirements specification referenced in the purchase order, and the practical consequence is that a nominal 100 mm plate can arrive meaningfully under nominal. For heavy-wall vessels, specifying restricted thickness tolerance and checking ultrasonic thickness maps on receipt avoids rework at the rolling stage. Flatness matters for the same reason: out-of-flat plate distorts the fit-up of a shell course and pushes weld prep out of alignment.

Ultrasonic examination is the standard quality gate for plate above roughly 30 mm. The order should state the acceptance class, the coverage, the probe frequency, and whether the examination is done before or after edge preparation. Lamination found at the edge is a different commercial problem from lamination found in the middle of the plate, and the specification needs to say what happens in each case. Z-direction quality, where the design has through-thickness stress at a welded T-joint, is ordered as a separate designation and is not implied by the plate grade.

Surface condition also deserves a line in the order. Scale, roll marks and minor discontinuities are normally acceptable within the limits of the general requirements, but grinding repairs deeper than the permitted depth change the effective thickness and must be recorded. A plate that has been extensively ground and then measured at nominal thickness is not at nominal thickness.

Typical Service Applications

The dominant application is hydroprocessing: hydrotreater and hydrocracker reactors, hot high-pressure separators, recycle gas exchangers and the associated piping. The second large group is coal gasification and synthesis gas equipment, where the combination of temperature, pressure and hydrogen partial pressure rules out carbon steel. Coke drums are a third, where the grade is selected not for steady-state creep but for thermal fatigue resistance under cyclic quench.

In power generation the grade appears in steam drums, headers and high-energy piping for subcritical and supercritical units, and in boiler components where the metal temperature exceeds the carbon steel limit. In petrochemical plants it shows up in reformer and platformer equipment, in ammonia synthesis loops and in sulphur recovery units where sulphidation resistance matters as much as strength.

Design strength at temperature should always be read from the applicable code stress tables rather than extrapolated from room-temperature tensile data. The allowable stress for 2.25Cr-1Mo falls with temperature in a way that is not linear, and the values in the code already account for creep and for the rupture data scatter that governs the high end of the range.

Purchasing Checklist and Acceptance Points

A complete enquiry for this grade should carry: the exact specification and grade, class, thickness and tolerance class, width and length, delivery condition, minimum tempering temperature, tensile and yield requirements, impact test temperature and energy where applicable, ultrasonic acceptance class, Z-direction requirement, step-cooling requirement, maximum residual element levels, and the required document package. Statements such as "SA387 Gr22 Cl2 plate, best quality" are unenforceable; the list above is enforceable at the receiving inspection.

The document package for a pressure vessel plate normally includes the mill test certificate with heat number and product analysis, the heat treatment record, the mechanical test results, the ultrasonic report, and the dimensional inspection. For Code work, the certificate has to be traceable to the plate marking, and the marking has to survive shipment. On arrival, check heat number against the certificate, verify thickness at a grid of points, confirm that the plate is not bowed beyond the tolerance, and hold the material until the impact and heat treatment records have been reviewed.

Two commercial traps recur. The first is a certificate that reports tensile strength just above the Class 2 minimum, which leaves no room for the softening that follows post-weld heat treatment. The second is a plate produced to the Grade 22 chemistry but delivered annealed and certified against Class 1, then offered as Class 2 because the chemistry "is the same". Class is a heat treatment and property designation, not a chemistry designation, and the two classes have different allowable stresses in the Code.

FAQ

Q: What is the difference between SA387 Grade 22 Class 1 and Class 2?
Class 1 is supplied annealed with 415–585 MPa tensile and 220 MPa minimum yield; Class 2 is normalized and tempered with 515–690 MPa tensile and 310 MPa minimum yield. The chemistry is the same, the heat treatment and allowable stress are not.

Q: What does the "22" in Grade 22 refer to?
It identifies the 2.25% Cr – 1% Mo composition family within ASTM A387/A387M, with chromium at 2.00–2.50% and molybdenum at 0.90–1.10% in the ladle analysis.

Q: Can SA387 Gr.22 Cl.2 plate be welded without preheat?
No. Preheat in the 200–250 °C range is normal practice for sections above about 25 mm, and the interpass temperature should be controlled. Unpreheated welding of this grade in thick sections produces hard, crack-sensitive heat-affected zones.

Q: Why is post-weld heat treatment mandatory for this grade?
Because the weld and heat-affected zone cool as untempered martensite or bainite. Tempering in the 690–710 °C range restores toughness, relieves residual stress and brings the joint properties back toward those of the normalized and tempered parent plate.

Q: What is temper embrittlement and how is it detected?
It is grain-boundary segregation of phosphorus and trace elements after long exposure or slow cooling through 375–575 °C, which raises the ductile-to-brittle transition temperature without changing tensile strength. It is detected by Charpy testing after a step-cooling treatment, not by tensile testing.

Q: What impact test temperature should be specified?
There is no single answer; the test temperature follows the minimum design metal temperature of the vessel, and it should be agreed with the design engineer and stated on the order together with the acceptance energy and specimen orientation.

Q: Is 15CrMoR to GB/T 713 a direct substitute?
It is the closest Chinese pressure vessel grade in the same 1.25Cr-0.5Mo to 2.25Cr-1Mo region, but it is a different specification with its own chemistry limits and allowable stresses. Substitution requires engineering approval and a documented comparison of properties at design temperature.

Send Inquiry