Mar 22, 2024 Leave a message

19Mn6 Boiler and Pressure Vessel Steel Plate: Grades and Use

What the 19Mn6 Designation Actually Covers

19Mn6 is a carbon-manganese steel plate grade written into the German boiler and pressure vessel code DIN 17155. The prefix 19 refers to the nominal carbon level expressed in hundredths of a percent, while the suffix 6 is a code value describing the manganese range rather than a direct manganese percentage. In purchasing practice the grade is understood as a normalised or hot-rolled plate intended for steam-raising and pressure-retaining equipment operating at elevated temperature, and it sits in the same technical space as Q345R under GB/T 713 and P355GH under EN 10028-2.

Because three separate code systems describe closely comparable products, the practical question for a vessel fabricator is not "which grade is stronger" but "which code governs the certificate, the impact test temperature, and the allowable stress the designer used". A plate purchased as 19Mn6 against DIN 17155 and a plate purchased as P355GH against EN 10028-2 will both satisfy a great many shell and head calculations, but they are not automatically interchangeable on a stamped vessel, because the impact energy basis, the permissible carbon equivalent and the permitted delivery condition can differ.

Standard Family and Cross-Code Equivalence

DIN 17155 was withdrawn as a German national standard and its content was carried into the European pressure vessel plate series. Suppliers therefore frequently quote 19Mn6 as a "historic" designation while certifying the steel to EN 10028-2 grade P355GH, or to GB/T 713 grade Q345R for deliveries from Asian mills. A buyer should read the certificate, not the trade name, and should confirm four items before accepting the equivalence: the steelmaking analysis, the delivery condition, the impact test temperature and energy, and the ultrasonic examination class.

The table below sets out the practical comparison. Values are typical specification ranges and must always be replaced by the actual certificate values for the heat being supplied.

Attribute 19Mn6 (DIN 17155) Q345R (GB/T 713) P355GH (EN 10028-2) SA516 Gr.70 (ASME)
Steel family C-Mn boiler plate C-Mn pressure vessel plate C-Mn pressure vessel plate C-Si pressure vessel plate
Nominal yield strength Approx. 315-355 MPa depending on thickness Approx. 345 MPa at 16 mm and below 355 MPa at 16 mm and below 260 MPa (38 ksi)
Tensile range Approx. 490-650 MPa Approx. 510-640 MPa 470-630 MPa 485-620 MPa
Typical delivery condition Hot rolled or normalised Hot rolled, normalised or TMCP by agreement Normalised, or TMCP with agreement As-rolled, normalised or stress relieved
Impact test basis Charpy V, room temperature as standard Charpy V, 0 degrees C as standard Charpy V, 20 degrees C for the base grade Charpy V, 0 degrees C typical for Gr.70
Typical plate thickness range 8-300 mm in the historic supply range 3-200 mm 6-250 mm 5-205 mm
Governing application code Historic German boiler code Pressure vessel code in China European pressure equipment ASME Section VIII Div. 1

Chemical Composition and Analysis Limits

The grade is deliberately lean. Carbon is held at or below roughly 0.20% to preserve weldability and toughness after normalising, manganese carries the strength, and residuals are tightly controlled because the steel is expected to remain ductile in the heat-affected zone of a thick-section weld. Phosphorus and sulphur are held at low levels so that through-thickness ductility is adequate for nozzle and manway welds made in the Z direction.

Element Typical requirement Why the limit matters in service
C 0.20% max, typically 0.15-0.20% Controls hardenability of the heat-affected zone and the ceiling on allowable stress
Si 0.50% max, usually 0.15-0.40% Deoxidation; excess silicon degrades toughness of the coarse-grain zone
Mn 0.90-1.40% typical for the historic grade Solid-solution strengthening; sets the tensile band
P 0.025% max Segregation and temper embrittlement risk in thick plate
S 0.015% max Lamellar tearing and hot cracking susceptibility
N 0.012% max, typically 0.009% max Free nitrogen ages the steel and lowers impact energy
Al (total) 0.020% min Fine-grain practice; without it the normalised toughness target is not repeatable
Nb, Ti, V Nb 0.05% max, Ti 0.03% max, V restricted Micro-alloy additions alter the normalising response and must be declared
CE (IIW) Commonly capped near 0.43-0.45 for thick sections Governs preheat and the risk of cold cracking

Two notes on the carbon equivalent. First, the calculation basis must be stated on the certificate, because carbon equivalent formulas differ between codes and the same heat can appear to pass or fail depending on which formula is applied. Second, a low carbon equivalent is not automatically good: if the mill achieves it by dropping manganese and compensating with micro-alloying, the normalising response and the elevated-temperature strength may shift, so the tensile test at the design temperature still has to be reviewed.

Mechanical Properties and the Thickness Effect

The published property band for 19Mn6 is a yield strength of roughly 295-355 MPa, a tensile strength of roughly 480-650 MPa, elongation at fracture of about 20% in the standard gauge length, and Charpy V-notch impact energy of about 31 J. These figures are quoted for a reference thickness and must not be read as a single flat guarantee across a 300 mm range.

Thickness changes the answer in two ways. The first is metallurgical: a 200 mm plate cools more slowly through the thickness during normalising, produces a coarser ferrite-pearlite structure at mid-thickness, and therefore tests lower in yield and impact than a 20 mm plate of the same analysis. Codes handle this by stepping the minimum yield and tensile requirements down as thickness increases, so a designer working at 150 mm must use the thick-section column, not the headline figure.

The second is procedural: for plates above roughly 40-50 mm the tensile test position moves from a near-surface location to a quarter-thickness or mid-thickness position, and the impact test set may be required from both the quarter-thickness and the mid-thickness location. A certificate that shows one tensile result with no test position stated is incomplete for a thick pressure part.

Yield strength: approximately 295-355 MPa, band dependent on thickness and delivery condition.

Tensile strength: approximately 480-650 MPa; the supplier must state whether the upper limit is mandatory.

Elongation: approximately 20% minimum in 50 mm gauge length, measured on a proportional specimen.

Impact: approximately 31 J Charpy V at the specified test temperature, average of three specimens, with a permitted single-specimen minimum.

Elevated-temperature proof strength: required where the design temperature exceeds roughly 200 degrees C; the Rp0.2 value at 300-400 degrees C is the governing number for the shell calculation, not the room-temperature yield.

Melting, Rolling and Delivery Condition

19Mn6 is produced by electric furnace or basic oxygen steelmaking followed by ladle refining, calcium treatment for inclusion shape control, and continuous casting into slab. The slab is reheated and rolled on a plate mill, then either left in the hot-rolled condition or normalised at roughly 890-930 degrees C with air cooling. Normalising is the default for anything that will be formed and stress relieved, because it removes the rolling texture, homogenises the banded ferrite-pearlite structure, and gives a reproducible impact result through the thickness.

Thermomechanically rolled delivery is also offered, and here the buyer must be careful. A TMCP plate of comparable strength is not a drop-in replacement for a normalised plate if the design assumes a normalised condition, because the designer's allowable stress and the fabricator's post-weld heat treatment cycle were selected around that assumption. Any change of delivery condition requires the design authority to re-confirm the allowable stress.

A typical order clause should specify: steelmaking route, fine-grain practice with aluminium, delivery condition, permitted surface condition, edge condition, ultrasonic examination class and coverage, marking method, and the document package. Leaving the delivery condition as "as rolled or normalised, at the mill's option" is the single most common cause of a rejected plate on arrival at the fabricator.

Forming, Welding and Post-Weld Heat Treatment

The grade forms readily. Cold forming of shells and heads to a fibre strain below about 5% is normally performed without intermediate heat treatment; beyond that, or where the plate thickness exceeds roughly 25 mm and the strain is severe, a normalising or stress-relieving treatment after forming is usual so that the deformed material retains its specified toughness. Hot forming is carried out in the range of roughly 900-1050 degrees C and must be followed by normalising, because air cooling from the forming temperature does not reproduce the specified microstructure.

Welding follows conventional carbon-manganese practice. For thicknesses below about 20 mm, welding without preheat is often acceptable at moderate carbon equivalent, but preheat of roughly 100-150 degrees C is standard for thicker sections, for high restraint joints, and for ambient temperatures below 5 degrees C or humidity above 80%. Low-hydrogen consumables are mandatory, matched to the tensile range of the parent plate, and the electrodes must be held in a controlled dry store.

Post-weld heat treatment is where most of the technical risk sits. The steel is susceptible to stress-relief cracking if the treatment is performed in a certain temperature window with a coarse-grain heat-affected zone, so the procedure should specify a charge temperature below roughly 400 degrees C, a controlled ramp, a hold at approximately 580-620 degrees C, a controlled cool, and a limitation on the number of cycles. Holding for an excessive time or repeating the cycle for repair welds can also reduce toughness, and the fabricator should track cumulative time at temperature for every seam.

Preheat: thickness and carbon-equivalent driven, typically 100-150 degrees C for sections above 25 mm.

Interpass temperature: capped, commonly at 250 degrees C, to avoid coarse-grain growth.

Heat input: kept within a qualified range; excessive input coarsens the coarse-grain zone and depresses impact energy.

Post-weld heat treatment: roughly 580-620 degrees C hold, with a documented ramp and cooling rate.

Repair: each repair counted and reported, with its own cumulative heat treatment record.

Applications and Where the Grade Stops Being the Right Choice

The classic applications are boiler drums, steam headers, shell courses of pressure vessels, heat exchanger shells, reactors, storage tanks, dished heads, flanges and pipe components in petrochemical and thermal power service. The grade is a good fit where the design metal temperature sits in the roughly -10 to +400 degrees C band, the wall is thick enough that strength matters, and the environment is not severely corrosive.

It is the wrong choice in three situations. Below roughly -20 degrees C, the carbon-manganese structure cannot deliver the required notch toughness and a low-temperature grade with nickel addition is needed instead. In wet hydrogen sulphide service, the plate requires hardness control and a qualified HIC or SSC test programme that a plain boiler grade does not carry. And in very thick sections with heavy nozzle reinforcement, the through-thickness ductility of a conventional plate may be insufficient, in which case a Z-quality plate with a specified reduction of area on a through-thickness tensile test should be ordered.

Inspection, Testing and Documentation at Delivery

Because the steel is used in pressure retention, the acceptance package matters as much as the analysis. A complete package for a 19Mn6 plate should contain the mill certificate with heat number and plate number traceable to the physical marking, the product analysis, the tensile and impact results with test positions and test temperature, the delivery condition, the ultrasonic examination report with the class and the scanning grid, dimensional and surface inspection results, and a statement of any repair by welding with the repair map.

Three verification steps are worth performing independently of the mill certificate. Confirm that the plate marking matches the certificate number by physical inspection at receiving. Confirm that the thickness measured at several points across the plate is within the ordered tolerance and that the plate is not wedge-shaped. And confirm that the impact test temperature on the certificate matches the design requirement rather than the mill's default, since a plate certified at room temperature will be rejected where the design calls for 0 degrees C or lower. Where the vessel is stamped, the authorised inspector may also require the test pieces to be witnessed or the results to come from a lot that has been witnessed, which has to be arranged at the order stage, not at delivery.

FAQ

Q: Is 19Mn6 the same steel as Q345R?
They occupy the same technical position as carbon-manganese pressure vessel plate, but they are not identical. 19Mn6 is defined by DIN 17155, Q345R by GB/T 713, and the two differ in impact test temperature, permitted analysis ranges and the thickness steps used to set minimum yield. Substitution requires the design authority's approval and a review of the allowable stress at the design temperature.

Q: What is the normal delivery condition for a 19Mn6 plate?
Hot rolled or normalised. Normalised is preferred for plate that will be cold formed, welded and post-weld heat treated, because it gives a uniform ferrite-pearlite structure and a repeatable Charpy result through the thickness. TMCP delivery is available but is not interchangeable with normalised delivery unless the designer re-approves the allowable stress.

Q: What thickness range can be supplied?
The historic supply range runs from about 8 mm to 300 mm. Above roughly 50 mm the test positions move towards mid-thickness and the minimum property requirements step down, so a designer working on a thick drum must use the thick-section values rather than the thin-plate headline figures.

Q: Why is ultrasonic examination specified for these plates?
Because laminations and internal discontinuities that are invisible on the surface can open up during forming or fail under pressure. The order should state the examination class, the coverage percentage and the acceptance criteria, and the report should identify the scanning grid so the fabricator can correlate any indication with a weld or nozzle location.

Q: What post-weld heat treatment temperature is used?
Typically a hold in the range of about 580-620 degrees C with controlled heating and cooling. The exact cycle is set by the qualified welding procedure and the vessel code, and the cumulative time at temperature must be tracked across production welds and repairs, because repeated or prolonged exposure reduces toughness.

Q: Can 19Mn6 be used at low temperature?
Not as a general rule below roughly -20 degrees C. The carbon-manganese composition cannot reliably deliver the required notch toughness at lower temperatures, and a nickel-bearing low-temperature grade with a certified impact test at the service temperature should be specified instead.

Send Inquiry

whatsapp

phone

Email

Inquiry