Due to the high cost of alloy wear-resistant plate, the shrinkage hole and yield of alloy wear-resistant plate after pouring are paid much attention by the majority of manufacturers. Statistics show that in the production of castings, using ordinary risers, the shrinkage volume of castings after solidification only accounts for 10% to 14% of the volume of the risers, and only 6% to 10% of the real castings are used for feeding. Using thermal insulation riser, the feeding efficiency of riser can be increased to 20% ~ 25%; The heat insulation riser, which integrates heat preservation and heating, can increase the feeding efficiency of the riser to 45%. Different from ordinary casting production, in the industrial melting production of alloy wear-resistant plate, most manufacturers are using ordinary thermal insulation risers for pouring, and the problems of large shrinkage holes and low yield are widespread. Therefore, using the production idea of casting for reference, the researchers designed and produced a heat and heat insulation riser integrating heat and heat preservation, and applied it to the production of cast alloy wear-resistant plate in VIDP type 4.5t vacuum induction melting furnace.
The heat source of the heat insulation riser is mainly achieved through the oxidation process of aluminum powder (typically thermite reaction). After effect comparison and cost analysis, the composition of the heat insulation riser is finally determined to be (w%) : Coal ash 10 ~ 20, aluminum powder 35 ~ 50, accelerant 2 ~ 10, resin 8 ~ 17, corundum powder 20 ~ 30, fiber powder 7 ~ 15, citric acid 0 ~ 1. In the experiment, Hafu cast iron mold with an inner cavity size of Φ360mm×2800mm was used, according to its matching cast iron riser sleeve inner cavity size Φ380mm×300mm.
Under the premise of not affecting the pouring, the design of small upper and large lower is selected for the heating and insulation riser. The longitudinal taper of the inner wall is 4°, which reduces the heat dissipation area of the liquid steel surface at the riser and helps to extend the solidification time of the liquid steel at the riser. It is also beneficial to reduce the adhesive force of the molten steel on the inner wall of the riser, so that the molten steel at the riser is easier to move down and feed due to the action of gravity; It is also conducive to improving the efficiency of stripping. The riser adopts the design of increasing the wall thickness as a whole, which is to ensure that the heating and insulation riser will heat up more fully when in contact with the liquid steel, and keep the heat longer, so as to extend the feeding time of the liquid steel. At the same time, with the extension of liquid time at the riser, it helps the inclusions in the liquid steel to float, and can play a role in purifying the liquid steel to a certain extent.
Experimental smelting alloy wear-resistant plates for Incoloy825, Inconel625 and Inconel718 each furnace. According to the amount of casting and the weight of the riser cut, the yield of vacuum ingot of the wear-resistant alloy plate of the third furnace is 96.1%, 95.9% and 95.0%, respectively, excluding the normal melting loss. The test results show that:
(1) The newly made heat insulation riser has high yield, good quality, high degree of mechanization, saving time and labor.
(2) The application of the newly made heating and insulation riser is conducive to increasing the solidification time of the alloy liquid at the riser, improving the feeding situation, and the primary shrinkage hole of the alloy ingot changes from deep V shape to U shape; The volume of the secondary shrinkage hole is greatly reduced, and the position of the secondary shrinkage hole is moved up obviously.
(3) Casting alloy wear-resistant plate in vacuum induction melting furnace, using heat insulation riser, can significantly improve the yield of vacuum ingot, the increase rate reached 2% ~ 3%, the cost reduction and efficiency is obvious.