ASTM A537 standard refers to pressure vessel plates, material in heat-treated, carbon-manganese silicon steel. Based on different strength and heat treatment, it ranges to Class 1, 2 and 3.
The maximum thickness under ASTM A537 Class 1 is 100 mm [4 inch], and 150 mm [6 inch] for Class 2 and Class 3.
A537 PVQ Steel Plate Chemical Composition:
|
Element |
Heat Analysis |
Product Analysis |
|---|---|---|
|
Carbon, max A |
0.24 |
|
|
Manganese (Tk≤40 mm or 1-1/2 in) |
0.70-1.35 |
0.64-1.46 |
|
Manganese B |
1.00-1.60 |
0.92-1.72 |
|
Phosphorus, max A |
0.025 |
|
|
Sulfur, max A |
0.025 |
|
|
Silicon |
0.15-0.50 |
0.13-0.55 |
|
Copper, max |
0.35 |
0.38 |
|
Nickel, max |
0.25 |
0.28 |
|
Chromium, max |
0.25 |
0.29 |
|
Molybdenum, max |
0.08 |
0.09 |
A537 Vessel Steel Plate Mechanical Property:
|
Mechanical Properties inch and [mm] |
Class 1 |
Class 2 |
Class 3 |
|---|---|---|---|
|
ksi [MPa] |
ksi [MPa] |
ksi [MPa] |
|
|
Tensile Strength |
|
|
|
|
2-1/2 in. and under |
70-90 |
80-100 |
80-100 |
|
[65 mm and under] |
[485-620] |
[550-690] |
[550-690] |
|
Over 2-1/2 to 4 in |
65-85 |
75-95 |
75-95 |
|
[Over 65 to 100mm] |
[450-585] |
[515-655] |
[515-655] |
|
Over 4 to 6 in |
A |
70-90 |
70-90 |
|
[Over 100 to 150 mm] |
A |
[485-620] |
[485-620] |
|
Yield strength, min: |
|
|
|
|
2-1/2 in. and under |
50 |
60 |
55 |
|
[65 mm and under] |
[345] |
[415] |
[380] |
|
Over 2-1/2 to 4 in |
45 |
55 |
50 |
|
[Over 65 to 100 mm] |
[310] |
[380] |
[345] |
|
Over 4 in to 6 in |
A |
46 |
40 |
|
[Over 100 to 150 mm] |
A |
[315] |
[275] |
|
Elongation in 2 in |
|||
|
[50 mm], min, %B |
22 |
22 |
22 |
|
4 in, [100 mm] and under |
A |
20 |
20 |
|
Over 4 in [100 mm] |
|||
|
Elongation in 8 in |
|||
|
[200 mm], min, %B |
18 |
C |
C |
Boiler Steel Plate Product Image: